Document zzdp495DNx7XJzmnZyv5JKw80

F, H, BEADLES B. B. FWiSf j . s. 1. T. BBEUER H. R. AYRES M, t. BYRON N. X. DRESS P. J. GRXPFXN H. E. JOHNSON R, J. BRAKE WXMINCSfON WILMINGTON WXLMJJWTON WILMINGTON CHICAGO SO. SAH FRAN. PHILADELPHIA EVERETT FLINT FT, MADISON h, l m R. H. BE; RUSSELL \j C. F. BGAN MX) ARLIN - C. B. SHERIDAN H,, F. TRUGHSESS Ho T, HUGHS A. Jo SteBHS Nl in miN mw i^ i LAB, J q _ p. KM-B E. X, DU PONT DE NEMOURS & COMPANY, INC, FABRICS & FINISHES DEPARTMENT FINISHES DIVISION PARLIN PLANT LABORATORY REPORT NO. 20 - -- -- ^FELOPMENT OF "47 PROCESS" REPLACEMENT FOR r m-m and m-m nmm* mmmm mMmmjm&jdm. i n:t Y `*f^'XX;X!X' X k*' 3a - 'vft .**' HiirfCi Copy: \ JWT /(IX3UI10II DAT! ISSUED; 8/12/57 PROJECT NO, * None PREPARED BYs /' AMOVED BYs "Planlsanager ` V I , N 29363 fmm rm$t immmtm mxm so,, 20 INTRODUCTION Currently MB-105 and MB-222 "Bulux" Furniture Flatting Mill Bases are manufactured at Partin for clear "Dulux" furniture products. To prevent color contamination, these mill bases are ground in small batches in porcelain lined mills using glass heads. Although 1956 production of mb-105 was only 13,600 gallons and MB-222 was 5,120 gallons, this 18,720 gallons inquired. production of 548 batches. Mot only was there an excessive number of batches, grit and gloss problems were constantly referred to the laboratory, m view of these factors and the favorable economies involved, "47 Process" manufacture of replacements for subject bases was In- v vestigated. mmmm The specific objectives of this Work were as follows* (1) To develop and evaluate "47 process" formulas to replace . currant MB-105 and MB-222, Vi'.:;; (2) lb determine the desirability of installing a "47 Process* unit at Parlln for the manufacture of developed replacements. (3) To formulate a single dispersion of G-222 santocel 0, in the interest of Simplification, which would replace both KE-222 and MB-105, mmm .m, s o t o s io n s In both MB-222 and MB-105, Santocel C (6-222), silicone dioxide is dispersed. Initial.batch grinds indicated that, while dispersion of this fine white fliafiy solid by W47~P" is not diffi- cult, metal discoloration of the clear products will result in For complete monthly production see JBxhibit III DUP030001324 2~ ~ conventional equipment manufacture. In an effort to reduce dis coloration, improve dispersion rate and reduce conversion cost, the amount of <1-222 in the "47-p" formulas was Increased *>0$$ over present ball mill formulations, The resultant "47-P" grind pro duced a relatively grit-free product, but was dark and dirty in color, "Teflon" discs were installed on the batch and continuous "47-P" units and MB-222 and MB-105 substitutes of good quality were produced. SX-J-12829 "47-P" replacement for MB-105 and SX-J-12828 "47-P" replacement for SB-222, were scaled-up in the 1/2-gallon bottom feed continuous "47-P" unit with little difficulty, let down formulas of these bases in RF-J-12830 replacement for KP-5294 and RP-J-12831 replacement for RF-5774 "Dulux" clear pro ducts, were made equal to respective standards. A single disper sion of G-222 for replacement of both SB-105 and MB-222 was deve loped, but will require more extensive evaluation to detenoine complete feasibility. Adoption of developed formulas will result in a grom savings* of $7,098 per year at Parlin and a reduction in flatting base inventory and storage of 50,700 lbs. per year. The savings is based on 1956 production and takes into consideration conver sion savings and shipping cost. At present it is more desirable to manufacture proposed "47-p" base at Philadelphia. Indications are that the savings will be realised with no sacrifice in prodnot quality and present plant grit and gloss problems will be essentially eliminated. AgglOM .TAKEN OR .PROPOSE!) In view of the favorable economies and the present diffi culties encountered by the plant with the use of MB-105 and MB-222, ^Savings make allowance for freight costs from Philadelphia to Parlin. DUP030001325 . -3it Is proposed that several 250~gallon batches of SX-cF-12828 and SX-J-12829 be manufactured at Philadelphia In the "47~P" nylon-disc unit, (order for 250 gallons of each base has been placed on Philadelphia). After scale-up formula alterations, these formulas should be adopted by the plant on a permanent basis, in view of the fact that Philadelphia has a "47-p" unit equipped with nylon discs, that yearly manufacture of proposed bases would utilize only 6.9# capacity of an 8-gallon "47-P" unit, that current cost of a conventional 8-gallon "47-P" unit installed is $15,000, and that Shipping cost from Philadelphia to Parlin would be only $647 per year, it is recoarasnded that the proposed bases be manufactured at Philadelphia until a "47-p" unit can be utilized at full capacity at parlin. Xt is further suggested that the consolidated base formulation, shown in Exhibit XX, and later discussed, be evaluated by the Marshall Laboratory as a replacement for MB-105 and MI-222. mmmm* Background 0-222, Santocel C, is a bulky porous material utilized in "Dulux" furniture finishes as a flatting agent, t o prevent particle agglomeration, this fine white solid must be dispersed before mixing into the furniture finish. MB-222 and MS-105 are flatting mill bases in which 0-222 is dispersed for use in "Dulux" HF-5200 and RP-5700 lines respectively. These bases are nuisance items be cause of the small batch manufacture and the necessity of grinding these clear intermediates in porcelain lined mills using glass beads. It was first suggested that the clears be manufactured by "47 process" in Philadelphia plant Laboratory Memorandum Report h o . 32 "settling of syloid 978, synthetic Silica in 'Dulux' Furni ture plate". Exhibits X and XX cover initial proposals for "4? Process" formulation and manufacture* DUP030001326 -4 Formulation During the development of "47-p '' replacements of t-222 and MB-105, it was found that by removing VO-332 nylon Solution ^ and Ml-718 or EC-721 Urea Formaldehyde Resins, the santoeel C con centration could be increased 59# for MB-105 and 60$ for MS-222* These simplified formulations resulted in better vehicle netting properties . The resin concentration was reduced one-third and the 0-222 to binder ratio was doubled (for exact figures see Exhibit VI). The resultant bases showed slight increases in viscosity and good settling stability. 0-222 has a tendency to form a soft gel or false body in concentrated solution, but the material is easily pumped by "47-2" equipment. "Jfcg!,. g..Scale.^u|> The two bases were ground in a standard n47-p" 1/2-gal. bottom feed continuous wait using ''Teflon" disc. The grind rate, one pass, of SX-J-12828 (replacement for MB-222) was 5 Ofttj and the rate for SX-J-12829 (replacement for MB-105) was 6,5 6$B. These rates suggest scale-up rates of 70 OPH and 90 OPH respectively in "47-p'' 8-gallon units. The rapid one pass grinds are desirable to prevent color contamination of the final product, Initial grinds in conventional batch "47-P" equipment resulted in dark dirty gray colored bases . Replacement of the metal disc with ''Teflon'' disc on the ''47-p" unit and increased concentration of G-222 in base fozmulas resulted in products equal to respective standards when let-down into RF-5294 and RF-5774 "Dulux" finished products. Base_Scale-up Data SX-J-12828 w 5.0 Sand to base ratio (volume) Temperature (*F.) 50/50 90-100 Dispersed Base Vise. (10 cup @25*0) 24" P/fc ratio (volume) 0. 3X-J-lg8S9 A 50/50 90-100 27" 0.070 DUP030001327 -5~ Evaluation of Developed Bases Investigation of let-down procedure revealed that hast results were obtained by stabilising the n4y-p" dispersion by slowly adding resin to it with the mixer miming, other methods of letting down SX-J-12828 andsx-J~12829 resulted la xeesalve grit caused by flocculation. The let-down formulas successfully developed are shown In Exhibit X? and V. Base evaluation is shown in Exhibits VI and TO. RF-5774 and RF-5294 products were chosen as critical products for test of flatting efficiency and metal contamination discoloration because of the large amount of base required in RF-5774 and frequent production difficulties encountered with RF-5294. it is significant that both standard and batch material had equal cloud and color tmabers, indicating that contamination was insignificant. Also, the "47-?" dispersed a-222 had good flatting efficiency as indicated by the gloss before vehicle adjustments. The 27 gloss of KF-J-12831 suggests that less 0-222 may be required when dispersed by "47-P'`, however, several producr tion batchee should be evaluated to establish this. Exhibit VII compares the flatting efficiencies of MB-105 and MB-222 versus the n47-P" bases developed, and further indicates that while the flatting efficiencies of MB-105 vs. sx-J-12829 show no significant difference, SX-J 12828 will produce a product 14 points flatter than its counterpart MB-222, at the same per cent of 0-222 concen tration. Pinal analysis will have to be made from sealed-up alignment batches DUP030001328 -6- Flatting Efficiency of MB-222 h -10`5 V&. SX-J-12828 and SX-J-128S9 (See Graph Exhibit VIXX) * 60 Gloss 60 Gloss 60 Gloss 60 Gloaa SX-J-12829 w -MS x 88 M2 | 20 10 r 6 3 89 | 12 7 4 89 80 U 24 11 4 Savings In the calculation of savings. Exhibits VXXI and XX, con version and flipping costs were considered. Based on 1956 produc tion, a conversion savings of $5,590 per year for MB-105 and $2,155 per year for MB-222 would be realized by adoption of proposed inter** mediates . The gross annual savings would be reduced to $7,098 be cause of a yearly freight cost of $647. The present annual produc tion of these mill bases is 145,974 lbs. compared to proposed "47-P" base production of 95,300 lbs. The savings in base storage would amount to 50,700 lbs. per year. The actual grind time required for mb-222 and MB-105 is 2190 hours per year as compared to proposed M47-p" formulas which require only 373 hours per year. She average batch size of MB-222 and MB-105 for 548 batches produced in 1956 was 34 gallons. The number of batches per year would be reduced from 548 to 37 if 500 gallon batches were produced by 8-gallon "4?-?" unit. Since production of the proposed bases would require 6.9# capacity* of an 8-gal. "47-P" unit, Philadelphia should manufacture the base. At present Philadelphia has the special "47-F* equipment in operation (see Exhibit I). . Shown m Figure XX, DUP030001329 Consolidation ofj@-222 and Mg-105 Since Ssntooel 0 is the media dispersed m both MB 105 and MB-222, it would be desirable from a simplification standpoint to replace these bases with a single dispersion that could be used in RF-5200 and RF-5T00 lines. These "Dulux" lines have a similar com position. The RF-5200 line resin binder consist of RL-255, Castor Oil Resin and RC-718 tfrea Formaldehyde Resin. The RP-5700 line resins are RC-6000 styrenated DCO Alkyd and crea Formaldehyde Resins RC-718 and RC-721. Both lines employ 0-222 dispersions as a flatting agent. Although RC-718 was common to both lines, investigation showed the wetting properties of this resin would not permit base formulation at a high 0-222 concentration. Therefore, a base which could replace MB-222 and MB-105 was developed using a combination of r c -6000 and RL-255 as wetting aids. Bet-downs of a batch "^7-PM grind into r f -5294 and RF-5774, produced products with gloss and . ? grit properties equal to respective standards. Small amounts of RC-6000 and RL-255 would be introduced into KF-5200 and HP-5700 lines respectively. The largest resin substitution in the RF-5200 line would be in RF-5283, Where 2.1$ of RL-255 would have to be substituted for RC-6000. Xn the BF-5700 line the largest resin substitution would be 2.8$ of RC-6000 for RL-255* the base formula is shown in Exhibit x, with a tabulation showing the neces sary resin changes in RF-5200 and RF-5700 lines in order to utilize the consolidated base, it may require substantial evaluation to determine the effect of the slight resin changes discussed, there fore, it is suggested that this evaluation he considered by the ^ Marshall Laboratory. DUP030001330 BYwrarp i EXHIBIT II EXHIBIT III EXHIBIT IV EXHIBIT V EXHIBIT VI EXHIBIT VII EXHIBIT VIII Ex h eft i*!* XX EXHIBIT X EXHIBIT XI EXHIBIT XU Philadelphia Plant Letter Furniture Flat Enamels" 'Duluxr PariIn Plant Letter " *4? process* Manufacture of MB-105 and MB-222" 1956 Production of MB-105 and MB-222 ^veXoped^eplaoemants for MB-105 Developed Replacements for MB-222 and RF-5774 Comparison of Base and Let-down properties Flatting Efficiency of MB-105 and MB-222 Vs, proposed "47-p" Replacements Conversion Cost and savings Based on 1956 Production Shipping cost, and per cent utilisation of 8-gallon "47-P" Unit Consolidated Base Formulation for MB-1Q5 and MB-222 SX-J-12828 "47-P" Laboratory Evaluation for Bottom Feed Manufacture for Philadelphia Alignment, SX-J-12828 "47-P" Laboratory Evaluation for Bottom Feed Manufacture for Philadelphia Alignment* DUP030001331 m $2 1 0 P C. B. SHERIDAN PARLIN Attentions J. W. Okonos COi E, T. Breuer, Wilra, E. A. Andre*, Lab, W. H. Pool, Lab, W*. PX,. WCoMl.iUo, LUaaWbb, Fhlla. plant Lab. File Philadelphia plant September 4, 1956 "DOLUX" FOT1TORK FLAT ENAMELS 47 PROCESS" IMIFACTOBE Res tour Aug. 28th, 1956 phone conversation with W,p, Colio, We are attaching a copy of Philadelphia plant Laboratory 's Memorandum #32 in 'which we recommended that consideration be given to manufacture of Santoeel 0 Type "Dulux" Furniture fiat at the Philadelphia plant by "47 Process* to reduce product manu facturing costs, A suggested "47 Process" formula for MB-105, "Dulux" flatting mill base, is included. The Philadelphia plant is currently manufacturing 32-5794, flatting base for RF-555, "Dulux" Satin Sheen varnish, by "47 process" using stainless steel - lined "47 Process" units and nylon grinding discs. Our original small scale, hand loaded equipment, has been supplanted by one 500-gallon premix tank, and two 13 1/2-gallon stainless steel- lined "47 Process" units mounted in tandem for the required two pass grind. The nylon discs are purchased from the Melarth Supply and Oasket Company, Tioga and Aramingo Avenues, Philadelphia, pa,, at a cost of approximately $45.00 each {12 inch diameter by 1-1/4 inch or 12 inch diameter by 3/8 inch). Since we have Just recently aligned on the new equipment, our production figures have varied, but it appears that We Will produce a minimum of 250 pounds of 32-5794 base per hour of unit operation. No accurate production figure for pounds of base per man hour is available since one man operates a number of units and time is charged to general "47 Process" grinding. Our loading time for a typical 3000-pound batch of base has been approximately 1-1/2 hrs. If interest in this process warrants, we would be happy to arrange for manufacture of a trial batoh on our existing equipment for your evaluation. JWBseak cossod DUP030001332 N 29363.01 0 0 p s C. Be SHERIDAN CGs E. T. Breuer, Wllm. H. P. Truehsesa Technical Area parlln, if, j, September 18, 1956 SIMPLIFICATION "4? PROCESS" MANUFACTURE OP MB-105 AND MB-222 ____________ _____ ___rmm___ ____________ _________ In December of 1955, 3. W. Bastian of the Philadelphia "B" Croup wrote a report recommending that Philadelphia manufacture MB-105 "Dulux" platting Mill Base for Parlln by "47 Process". Phis report, Philadelphia Plant Laboratory Btoorandum Report No. 32, indicated that satisfactory product had been made at Phlla. by "47 Process" and that savings of ten cents a gallon were possible. The suggested Philadelphia formula calls for a two pass grind in stainless steel lined units using nylon grinding discs, the special equipment being required to prevent color contamination. Now that we have a laboratory scale "47 Process" unit and will eventually obtain coma for plant use, it is recommended that work be carried out to develop satisfactory "47 Process" formulas for MR-105 and *-222, both of which are currently mad by glass bead grinding. In 1955 m made 496 batches of MB-105 at an average batch size of 268 lbs. and in the first eight months of 1956 we have made 201 batches. As for the MB-222 we made 187 batches in 1955 and 82 in the first eight months of 1956, each of an average batch size of 266 lbs. The attached tabulation shows our production by month for 1955 and 1956 up to September 1, and Shows that in 1955 we mads as many as 152 batches of the two mill bases in one month. This required 608 hours of grinding time alone without even considering loading and unloading time. This same amount could be made in I63 hours of grinding time in a "47 Process" unit and could be automatically pumped to a stor age tank, thus eliminating unloading costs. Parlln cost group calculations indicate that the savings should be ten to twenty cents a gallon on MB-105. The savings on MB-222 would, of course, be similar. In view of the simplified manufacturing procedure and large savings possible, it is recommended that the suggested development work be carried out in conjunction with the other "47 Process" work aimed at replacing the "SOW-49 Process" formulas for certain 253-line tinting solutions. 3, W, GKDNOS jWSUMCN oc*eod N 29363.02 DUP030001333 mmsLm 1956 PRODUCTION OP MB-105 AMD MB-222 mo n t h March April AllgUSt September October November December Total fe|Qg, FOMM 21 5,341 6 1,589 4,028 14,871 10,633 22 5,921 42 11,256 42 11,244 54 14,414 57 15,277 11,462 398 106,026 mmMB-222 fe.BWCHa 20 5,274 1,326 2 7 6,469 1,872 16 4,286 10 2,679 8 2,122 42 U,228 13 150 39,978 MB-105 Avg.batch size MB-105 lbs. * 106, batches Avg.batch size MB-105 gal. 266 34 gal/bafceh Avg.batch size mb-222 its. * * 266#/ioafc;eh atches Avg.batch size MB-222 gal. 266/bafcch 34 gal/batch \y/!< " ' " DUP030001334 N 29363.03 sxrj>gg822.imumrnjmMzrn^ f^ion H-12 KG-6000 in.Jii 29.0 25*0 Portion "47 Process11 Add in order shown and mix 10 mins. 8~gal. "47-P" mlt Kates 50 GPH temps 0-120F. Add lowly to musing Wt/Oals 7.96 mixer, mix 1 hour,then grind. HP-J-12830 {Replacement for RP-5E9M *!rtt Position s x -j -12829 H-583 BG-6000 JL 6.4 1.1 44.5 Second portion HC-718 H-136 H-12 30.6 1:1 V8-33S X.7 Add slowly to running wt/oal. 7.97 mixer in order listed. Vises 45-$5w 7 cup Mix 15 mins. Total Solidss 40.0 Add slowly to running mixer in order listed. Mix 20 mins. Adjust to gloss third portion H-583 Add to adjust viscosity o > DUP030001335 wnaeoBL H-202 H-12 RL-255 0-222 3lJ^ss2ai: 37.0 30.0 18.0 Add and mix 10 mins. 15.0 Add, mix 1 in?, then grind 8-gal "47-F* Unit Hats* 50 OIK Temps 90-120F. Sand to Bases 50s50 "Teflon" Oise required Total Solidss 26.8 Wt/Gals 7.7 .. S3KTH-202 BJj-255 gStpiid,,portion RC-718 KC-721 TO-: a-i H-12 K38 Third Portion H-202 U3 Add slowly to Wt/Gals 1.0 running mixer. in Vises ,, _M 7 i.o order listed. Total Solids? 43.8 Mix 15 mins. 26.8 1:1 5:5 Add slowly to running mixer in order listed. Mix 20 mins. ^Adjust to gloss 4,5 Adjust to vise. DUP030001336 i s common p ra c tic e t o add more m i l l base o r re s in to a d ju st to proper gloss. **01oss taken before any adjustm ent made. I t *$hare is no s p e c ific a tio n fo r cloud, b u t is tested fo r contam ination. Si I 01 C*Mn\oVmifiHO in fHib 01 rt t* O s K CO gl & -i *H op$ _ <X> gl $243 co e* Si i -`t,lr | ^C0.. 00.?L ojcinm<thnSoih*o < oIO^Nf' Rfe fw *rt TO 0^o1w* cifwootn ' H'8oV a> Of I pin oi frf ' S* O rt jl s oo |toils >00000 DUP030001337 So t ~s w <m sse-aw 1 VIII msmmjmjmMmrnMmLMjmj Conversion cost foe Ball Mill * 0.072|/# Conversion cost for "47 process" 0.029$/# (1) #0-222 dispersed la f~105 *106,026# X 0.093 9850# (2) #0-222 dispersed In MB-222 *39,94$# x 0.094 3760# (3) #"47-?" Base to replace MB-105 ** 70,300# (4) #"47-P*' Base to replace MB-222 (5) Base s ^ZSM (6) Conversion cost MB-105 and MB-222 ** 0.072$/#(l06,026# + 39,94$#) . 410,510 (7) Conversion coat SX-J-12828 & SX-J-12829 0.029$/# (25,000# + 70,300#) 4 2,765 ($) Conversion savings (6) - (7) ** 410,510 - 42,765 tzm *3ee Exhibit ill DUP030001339 mvs mx&mk'siox Baalgl^ljrg., Freight cost from Philadelphia to Parlin 0.006$/# (1) #Base shipped (2) #Drums for Base 95,300# 12,600# (3) Total shipping weight 107,900# 4$ Total shipping cost 107,90c# X 0*006$/# * $647 (5) *Net savings Conversion savings -shipping cost #7,745 * #647 #7,098 iMm&x Average production rate *. 50 QFH Average waight/gallon * 7.8#/gal. Total available grinding hows * 3,560 hrs/year Capacity of 8-gal unit <* 50 gal/hr. x 7.8#/sel. X 3,560 hrs. 1,390,000# Total proposed base production * 95,300# from Exhibit 17 $> of 8-gal. unit utilised by proposed bases x 100 ' M. provided Intermediate la manufactured in Philadelphia Allows down time for maintenance, cleaning, loading and premixing. DUP030001340 MmAg-105 Mm MB-222 Consolidated Baa Formula* girst Portion I-l?2 SC-6000 RL-255 Second portion <2-222 120 19.0 25.0 12.0 10.0 -^X-^S2SSSU Total Solidsj 25.3^ Suggested Grind Data 8-sal, w 47-P" Unit Add in order shown. t*llon Mix 10 aains. gate* 50 OPH TsaiPl 90-120*P. Sand to Bases has not been scaled-up in 1/2 -gal. continuous unit. 5278 OOMSOL.BASE 1.7 18.0 1.7 21.3 20.0 5.0 8.0 is:? 19.3 6,1 21.3 11.3 17*3 20.6 6.3 23.3 20.7 6.6 20.7 % RL-255 **$ of RL-255 replaced by SC-6000 :..UyS;s 'M. ' -Vx': DUP030001341 CODE? SX~<?-12828 (Replacement for MB-222) TITLE* "Dulux" Bass P/L r a t io s 0.074 by volume SAND LOADS 2300 grams BATE (Oal/Br) * 5,0 OFH SAND LEVELClnchea); 2.5 inches from top LIQUID LEVELClnchea)t 3*0 inches from top SAND/feASE TEMP,(F.) t 100-110*F. BASE TEMP. AT TROUGH ("?.)* 90~100*F. RESIN SOLIDS ()* 10.80 DISPERSED BASE V33C* 24" 10 Oiap ft 25 C. REMARKSs (with regard to skinning tendency, false body offset on flow in trotyl, ete.) Satisfactory operation in all respects. DUP03Q001342 "4? PROCESS* LABORATORY EVALUATION aj|* AMMWIA aMAWIM M MMM A A CODE? SX-J-12829 (Replacement for MB-1Q5) TITLE? "BuXux" platting Base P/L RATIO? 0.0?0 by volos SAND 10AD? 2300 grams SATE (Gal/Nr) 6.5 CPH SAND BEVEL(Itt.) 2.5 inches from top LIQUID LEVEL(X.)3.0 inehea from top SAND/5&ASB CSNP.C^v ) ? 100 - XXQF. b a s s y s mp ,a t t r o u g h c^)* 90 - ioo*p. RESIN SOLIDS (#) 8 12.$* DISPERSED BASE VXSCt 27" 10 Cup@ 25 C. REMARKS? (With regard to skinning tendency, false body effect on flow In trough, to.) Satisfactory operation in all respects* DUP030001343