Document zoQNZwmZVdQkeEn84KqeNX1Qg
1-1-35 Supersedes 11-20-33
( SWAM CHEMICAL COMPANY
f AROCLOR EMULSION FOIMULA
/
/
/
/
/
I
16 pounds of Aroclor 8 pounds of Water
16 ounces of Stearic Acid 4 ounces of Triethanolamine
The Aroclor is heated to a workable viscosity above 180 degrees F.
and the stearic acid is added and completely stirred in. The water
is heated to 207 degrees F. and the triethanolamine added and
thoroughly stirred in. fAfter both of these operations have been
carried out, the Aroclor-stearic acid combination is poured into
the water mixture while the latter is well agitated and then the
whole mixture is processed through a colloid mill. Good results
1 may even be obtained without the use of a colloid mill, provided
t the mixture is agitated with a high-speed emulsifying stirrer.
(
* DSW 312180
STLCOPCB4072166