Document zd0bQbD12BYGrG3Kgxx0YegG0

/& A i'` rn(CtiX'izi& ' /. /Ay # >*W FF$f F/'<: (%'*', (:/M. &(J2M($!' 0 ZZl*1'0 TOWOLDMON0027160 WATER_PCB-00011629 CONTENTS Synthetic-Resin Adhesives--A Growing Market...._____................ 2 Development of Synthetic-Resin Adheyves........................ 3 Emulsion Adhesives................................................ 3 Polyvinyl Acetate Adhesives............................... 4 Monsanto Plasticizers................ 4 Monsanto Resin Additives.................................................... 6 Monsanto Preservatives end Odor-masking Agents......... ........................ 6 Adhesives................................................... Polystyrene Adhesives__ ...._______ 6 10 Hot-Melt Adhesives............ .............. .10 Deleyed-Tack Adhesives................................... 13 Solution Adhesives_________ ...___ ................... ..15 Vinyl Adhesives................. ............................................................ ................15 Nitrocellulose Adhesives........................ ...16 Cellulosic Adhesives................................... 16 Polyurethane Adhesives.......................... 18 Chlorinated-Rubber Adhesives........... ..................... 18 Zein Adhesives.......................... 19 . Pressure-Sensitive Adhesives................................................_______19 Adhesive Primers............__ ......... ...21 Miscellaneous Adhesives.......................................................................... 22 Toxicology........................................................................................................................... 23 Ingredient Index.........................................................i.................... .....................24 Technical Literature............................. ...26 Shipping................... 28 fMhlnftonUInrttirtlnlitebtttnitrMd mncommintfitlon Is uu inyuoducl ineonlUctallti fi, MONSANTO MAKES NO WARRANTIES AS TO THE flTNESS OR MERCHANTABILITY or ANY rROOOCTS RtfCRRIP TO. *o iirnlM of utivlttlory rottiiu Ifom umnt upon tonWwOinlwmiUon or r*c#mmh4i1K''U.ind0iKlln>llirt>i% tornymYiir>jio*w | TOWOLDMON0027161 WATER_PCB-00011630 J_____________________________ :_____________________ :__________ I____SYNTHETIC-RESIN ADHESIVES- ft CROWIHG MftRKET Consumption of synthetic-resin adhesives is rapidly expanding both because of continuing dis placement of older gluing materials in steadily-growing uses Bnd because of the introduction of many new applications for which conventional adhesives are unsuitable. Superior performance I of the synthetic-resin adhesives has enabled them to supplant conventional adhesives based on natural products in many large-volurrie applications. Wide-spread and increasing usage of synthctic-resin adhesives is foreseen in such diverse industries as the following: Shoe manufacturing Book binding Paper-bag and folding-box-carton manufacturing Food-coniainer production Food packaging (labeling, sealing, wrapping, etc.) Tobacco packaging Specialty product packaging Automobile production Building construction Use of the proper plasticizer in synthetic-resin adhesives -- to best accomplish the desired pur- I pose ol the adhesive for its intended application -- is extremely important. The plasticizer in an adhesive formulation improves film formation; imparts tack, flexibility, and gloss; decreases1 drying time; and lowers production costs. I More synthetic-resin adhesives are used today than ever before because: Synthetic-resin adhesives adapt well to high-speed sealing and labeling machines, thereby increasing production rates. Synthetic-resin adhesives are cleaner, easier to use. They keep maintenance costs down. Synthetic-resin adhesives resist deterioration caused by water, light, and fungus much better than the usual adhesives based on natural proteinaceous materials. Adhesive emulsions require no volatile, toxic, or flammable solvents. Emulsion properties are easily adjusted and controlled. . Monsanto Chemical Company, a major supplier of plasticizers for synthetic-resin adhesives, of fers plasticizers that are efficient, heat and light stable, and non-toxic. Lack of toxicity is es pecially important now in food applications because of the 1958 amendment to the Federal Pure Food, Drug, and Cosmetic Act. Monsanto plasticizers impart excellent grease resistance and heat 2 0 C TOWOLDMON0027162 WATER_PCB-00011631 scalability to the adhesive. Because of the great, variety of Monsanto plasticizers, customers can realize lower costs by taking advantage of mixed shipments. This bulletin suggests typical formulations for various adhesive applications and describes the benefits to be derived from the use of plasticizers in synthetic-resin adhesives. If you need addttional assistance, experienced Monsanto technical representatives are always ready to help you with your special formulation problems. Since Monsanto does not have a vested interest in any particular plasticizer, you are assured of advice directed toward achievement of the best poszible performance of your product DEVELOPMENT OF SYNTHETIC-RESIN ADHESIVES Not long ago industrial users or consumers could choose among only a few naturally derived materials for their adhesive applications. Constant industrial demand for adhesives with greater strength, faster tack, and greater versatility for bonding many types of surfaces forced the de velopment of synthetic-resin adhesives. With the great number of excellent adhesives now avail able, both industry and consumers have a much wider choice and are more likely to obtain suitable adhesives to fill specialized needs. Only synthetic-resin adhesives are able to tolerate extreme exposure conditions. They withstand temperatures that quickly destroy natural materials, and they bond surfaces -- such as rubber and metal -- that normally defy bonding. From 1946 to 1956, synthetic-resin adhesives gained dominance among adhesives in major construction. For nearly any fastening job, a good syn thetic-resin adhesive is now available. Synthetic-resin adhesives commonly used are based on vinyl polymers (polyviny acetate, poly vinyl alcohol, and polyvinyl chloride); on condensation resins (urea-formaldehyde, melamineformaldehyde, phenol-formaldehyde, resorcinol-formaldehyde); on cellulose derivatives; polyes ters; elastomers; and epoxies. Addition of plasticizers generally modifies an adhesive to suit a particular need. TYPES OF RESIN-ADHESIVE FORMULATIONS The major types of plasticized synthetic-resin-adhesive formulations are emulsion, hot-melt, delaycd-tack, solution, pressure-sensitive, and adhesive primers or coatings. These types will be discussed in order. Suppliers of special ingredients are listed at the end of this bulletin. EMULSION ADHESIVES Resin-emulsion adhesives are emulsions of plasticized or unplasticized resins dispersed in a water base. They offer the advantages of reduced fire and toxicity hazard because of the elimi nation of volatile, flammable, and possibly toxic solvents. 02225*0 TOWOLDMON0027163 WATER_PCB-00011 POLYVINYL ACETATE ADHESIVES The widely-used polyvinyl acetate-emulsion adhesives possess quick tack, good adhesion to many yrfoces, grease resistance, non-toxicity, and many other desirable features. . Mcwanto PlasticTiers for polyvinyl acetate-emulsion adhesives Monsanto liquid plasticizers most commonly used in the polyvinyl acetate-emulsion adhesives lire Santicizer* 160, dibutyl phthalate, Arcc/or* 1221, Aroclor 1232, Aroclor 1242, dimethyl pblhalate, diethyl phthalate, tricresyl phosphate, Santicizer 140, Santicizer 141, Santicizer M-17, Santicizer B-16, Santicizer E-15, and Santicizer 8. Dibutyl phthalate imparts good flexibility and softening action with relatively low volatility. Sontlcher 160 is considered better than dibutyl phthalate in most applications because of lower volatility, improved moisture resistance, and film toughness. Diethyl phthalate is used for fast-tack, non-toxic applications. The Aroclor plasticizers impart quick tack, good adhesion to many surfaces, and are widely used in commercial adhesives either as extender plasticizers or alone to make versatile, lowcost adhesives. Dimethyl phthalate is preferred in polyvinyl acetate adhesives for bonding cellulose acetate film or sheeting because of its better solvency action on the cellulose acetate. Uses for this type of adhesive include covering cut-out windows in cartons or for laminating paper. Santicizer 140, Santicizer 141, and tricresyl phosphate are used when flame resistance, oil re sistance, and low volatility are desired. Santicizer 141 is most efficient in polyvinyl acetate adhesives, followed by Santicizer 140 and tricresyl phosphate. For bonding overlays of paper, Santicizer M-17 is frequently used for its superior light sta bility, quick tack, and solvency on cellulose acetate. Santicizer 8 imparts excellent grease resistance, good flow and wetting action, and improves the bonding of rubber to metal. ' Monsanto's solid plasticizers, Santicizer 1-H, Santicizer 9, diphenyl phthalate, dicydohexyl phthalale, and Aroclor 5460, are frequently used in polyvinyl acetate-emulsion adhesives to Impart better heat-sealing characteristics. They also improve moisture and solvent resistance. For nontoxic adhesives, Santicizer B-16, Santicker E-15, Santicizer 141, and diethyl phthalate have been accepted by the U. S. Bureau of Animal Industry and the Food and Drug Admini stration. Typical illustrations of the use of these products include adhesives for food-wrapping films, boxboard manufacture, and envelope adhesives. Table I on page 5 lists performance data of Monsanto plasticizers in polyvinyl acetate. 'Arcelor; Saniiciser; Monsanto Chemical Company trademarks. Regiftered in U.S. Patent Office. 4 e 0; Ct TOWOLDMON0027164 WATER_PCB-0001 TsUs I. PERFORMANCE OF MONSANTO PlASTJCtZKS IN POLYVINYL ACETATE-EMULSION ADHESIVES Ptasfter2rt* . Aroclor 1221 Aroctor 1232 Aroctor 1242 Triphenyl Phosphate Tricresyl Phosphate Dimethyl Phthalate Diethyl Phthalate Dibutyl Phthalate Diphenyl Phthalate Santieizer B-16 Santieizer M-17 Santieizer 1-H Santieizer 8 Santieizer 9 Santieizer 140 Santieizer 141 Santieizer 160 Volatility 20 Hours at 87 C (Activated Carbon) (per cent) 5.Z 4.8 4.4 2.0 0.7S 5.6 4.8 4.4 . 5.9 2.2 3.6 1.5 3.6 3.1 1.2 1.8 2.1 Low-Temp. Flexibility (Modified dash it Berg Test) (q -5.0 4.0 5.3 5.7 3.6 -1.6 -S.0 -6.1 -- -3.9 1.5 -- 6.4 -- 5.0 --3.3 1.9 Oil Extraction--Weight toss After 24 Hours at Room Temperature (per cent) Kerosene 0.63 0.54 0.57 0.02 0.16 0.92 0.85 0.59 131 0.08 0.19 0.96 0.43 1.13 0.15 0.17 0.20 Peanut Ot! Cotton Seed Oil _. -- -- 0.37 038 0.75 0/63 0.51 0.90 0.46 0.50 0.36 0.60 0.57 034 0.42 039 _ -- > .-- 038 0.46 0.93 t 032 0.59 0.98 036 0.48 0.53 0.64 0.63 036 031 034 'Formulation: 11 part? flaNkmr m 100 pvt* Celvj $-55 (polyvinyl acetate) emulsion. F3m thickness 0.040 inch. . TOWOLDMON0027165 WATER_PCB-00011634 Monsanto Resin Additives for Polyvinly Acetate Adhesives I Monsanto Industrial resins, Sontolite* MHP and Sontolite MS-80%, when used to modify polyl Vinyl acetate adhesives, give a very tough but flexible product. They Impart quick tack ana adhesion to a wide variety of surfaces. Normally, they are compounded with a liquid plasii- tber, such as dibutyl phthalate or Santtcher 160, or with an eutectic mixture (1:1) of dibuty l pbthalate and triphenyl phosphate. * . The Sontolite resins are especially useful to bond cellophane or aluminum foil to paper. Monsanto Preservatives and Odor-Matling Agents for Polyvinyl Acetate Adhesives Monsanto supplies a complete tine of industrial preservatives including Simfohrife*, Monsanto':. Penta (pentachlorophenoi), and technical sodium benzoate. These materials are useful in pre venting fungus attack on the adhesive if natural materials, subject to fungus attack, are incor porated In the formulation. Monsanto odor-masking agents for polyvinyl acetate include Santomask* II, methyl salicylate Coumarin, and vanillin. Literature on these products is available on request. Polyvinyl Acetate-Adhesive Formulations Polyvinyl acetate-emulsion adhesives range in complexity from simple blends of polyvinyl ac<tate and plasticizer to more complex formulations involving many ingredients. formula No. 1, presented as a guide to general polyvinyl acetate-emulsion adhesives, illustrate^ the types and range of concentrations of ingredients that may be Incorporated for various e< Jjesive applications. (An index of formulation ingredients and their suppliers begins on page 24i] Formula I--Genera! Polyvinyl Acetate-Emulsion Adhesive Ingredient -Polyvinyl acetate emulsion ($5% solids) Plasticizer ;Ciay filler -Cooked starch or dextrine Preservative Stabilizer . Wetting Agent Secondary Water Defoamer - Odorant (masking agent) by Weight 100 10 50 0-30 0-1000 0-2 0-2 0-0.2 0-100 0-2 0-1 Somobriif. &ant#mas\,: Monsanto Chemical Company trademark?. Registered in U.S. Patent Office'. * 0222546 II I TOWOLDMON0027166 WATER_PCB-00011635 [ Formulas 2 through 6 Illustrate five of the most widely used applications for polyvinyl acetate adhesives. Formula 2---Quick-Tack Polyvinyl. Acetate-Emulsion Adhesive Ingredient Gclva S-S5 polyvinyl acetate emulsion Sonticher 160 Santicfoer 8 Water Farts by Weight 100 12 12 9.0 Formula 3--Polyvinyl Acetate Adhesive or Glue tor Wood Ingredient . ' Gelva S-55 polyvinyl acetate emulsion Sonticizer 160 or dibutyl phthalate Water Parts by Weight 95 3 2 Formula 4--Low-Cost, Quick-Tack Polyvinyl Acetate Adhesive Ingredient - Gelva $-55 polyvinyl acetate emulsion Arcelor 1232 Parts by Weight 100 11 Formula 6--Typical Polyvinyl Acetate Combining Adhesive Ingredient Polyco 117 H Dibutyl phthalate Water Solids content 62.5 Viscosity 2500-3000 centipoises Parts by Weight 64.9 26.6 8.5 0**2547 | TOWOLDMON0027167 WATER_PCB-00011636 Formula 6 Illustrates a Polyvinyl Acetate Adhesive for Padding Ingredient Parts by Weight Polyco 117-H Trlcresyl phosphate Water Polyco 118 - 42.3 . 11.6 4,6 41.5 1 Add Polyco 118 to 117-H with good agitation. Then slowly add trlcresyl phosphate with high-speed agitation. Blend water slowly. Solids content Viscosity 40 4000-5000 ccntipoises For bonding moisture-proof cellophane to aluminum foil or paper or for bonding aluminum foil to paper, Formula 7 is especially useful. Adhesion develops rapidly, and good bond strength is maintained at high temperatures. Formula 7--Polyvinyl Acetate-Emulsion Adhesive for Cellophane, Aluminum Poll, and Paper Ingredient Oclva S-55 polyvinyl acetate emulsion Santicher 160 Sonlolite MS-80% Water ' Parts by Weight 100 9 15.5 13.4 Polyvinyl acetate emulsions are used for grease-proof coatings on paper. Although Formula 8, for "flatboard," and Formula 9, for "flexible board," are not used in true adhesive applications, they arc Included to show the versatility of Monsanto's plasticizers in polyvinyl acetate for mulations. , Ingredient Parts by Weight * Formula 8 Formula 9 Flvacet 81-900 polyvinyl acetate emulsion Santicher 141 York Whiting No. 7, superfine calcium carbonate Futile titanium dioxide ' Tamol 731 dispersing agent (25% aq. soln.) Elvanol 71-30 polyvinyl alcohol (10% aq. soln.) Poly-G P-1200 polypropylene glycol Water 100.0 8.25 119.25 13.25 2.1 30.0 1.0 34.0 100.0 13.75 95.75 10.75 ID 30.0 1.0 34.0 0222**8 TOWOLDMON0027168 WATER_PCB-00011637 / ' *olids ' 'finWy (26 C), centipolses 1 / ' (/.(it-to-blndei- ratio resln-to-PVA resin ratio V/' fesin-to-plasticizer ratio Formula 8 6$ 1600 2:1 18:1 6.6:1 Formula 9 65 2700 1.5:1 18:1 4:1 -pare these grease-proof-coatings, the following procedure is suggested: ..jffr a stock solution by mixing polyvinyl alcohol in water at room temperature. Heat //) to 40 minutes at 185 to 190 F. The w^ter required to adjust the solids content ' *I,# added Itno ttlhiiics csltnorclkr tsnolliuittiAionn, jjptje stirring, and add the Santtcher 141, Poly-G P-1200 dcfoamant, and Tamol 731 ////^t-<Hspcrsant solution. 1 ^i t)# pigments, stirring until dispersion is complete. /' polyvinyl acetate emulsion, and stir until a homogenous mixture is obtained. y/*jstant coating for wrapping papers, such as used for bakery goods, is illustrated In ^ f/j. The composition may be applied with a roller coater provided with a smoothing S/yr a uniform, continuous film. About 140 F is required for optimum film formation, v. /y f& used as a laminating adhesive. Formula l(^--Polyvinyl Acetate Grease-Resistant Paper Coating fji}*. 81*900 polyvinyl acetate emulsion - B-16 ( /' dioxide Irt' Parts by Weight 100 3.5 7.0 15-30 0-5 \f / *^phcalions, incorporation of a solid plasticiser to provide rapid heat-scaling is de- ulas 11, 12, and 13 illustrate the technique of dispersing diphenyl phthalate, Soni(( * '</ jnd triphenyl phosphate, respectively, in water, for convenient incorporation into t| ss/l atcetate adhesive. f yji/t phtholale S /trsf l-H | :T P|,0SPh*"! T, \l " yj./pyolildonc (i /^yiyjnethylcellulose Formula II 100 100 4.7 1.3 Part* by Weight Formula 12 100 100 4.4 1.3 Formula 13 100 100 4.4 1.3 0222549 W'miWlUFW' | TOWOLDMON0027169 WATER PCB-00011638 The procedure for preparation of these formulations Is as follows: 1. Grind the solid plasticizer with dry ice to the desired particle size. The dry ice prevehls coagulation of the solid plasticizer as a result of softening from frictional heat. 2. Add the thickening agents to the water, and agitate this mixture until solution is effected. 3. Slowly add the solid plasticizer to the water-thickener mixture with good agitation. This dispersion may be used in any desired polyvinyl acetate-emulsion formulation. POLYSTYRENE-EMULSION ADHESIVES Use of polystyrene-emulsion adhesives is increasing. Santickcr 160, HB-40*} diethyl phthalate, dibutyl phthalate, Aroclot 1242, Aroclor 124$, and Aroclor 1254 are extensively used as plas ticizers for this resin in adhesive emulsions. Formula 14 illustrates a basic styrene-emulsion adhesive that is stable and has a high degree of wet tack. The caseinate imparts stability, wet tack, and film toughness. These properties may be varied by alteration of the caseinate concentration. Formula 14--Styrene-Emulsion Adhesive Ingredient Parts by Weight Luslrex* Styrene 601-40 100 HB-40 13.0 Diethyl phthalate 5.0 Triton XI55 2.5 Ammonium caseinate, 15% aqueous - 34.0 HOT-MELT ADHESIVES ] I Hot-melt adhesives are utilized because they set rapidly after application. The molten adhesive Is applied to the materials to be joined; the bond sets before the adhesive is cool. Plasticizers play an important part in the successful manufacturing and application of hot-melt adhesives. Liquid plasticizers, such as Santicher M-17, Santicizer 160, dibutyl phthalate, Sonticker B-16, and the Aroclor liquids, are frequently used. Solid plasticizers, such as diphenyl phthalate, dicyclohexyl phthalate, Santicher 1-H, Santicizer 9, and Aroclot 5460, are also utilized in many applications, since they melt at the processing Lustrex; Monsanto Chemical Company trademarks. Registered in U. S. Patent Office. I TOWOLDMON0027170 WATER_PCB-00011639 i o 9 temperature of the hot-melt adhesive. Upon application of the adhesive to the materials to be bonded, these plasticizers solidify as the temperature is reduced, thereby overcoming the prob lem of excessive softness frequently encountered with hot-melt adhesives. Formulas 15 and 16 represent two starting formulations for bookbinding adhesives. Formula 15 Ingredient Kevlllac Hard Resin Santkher 160 Paraffin Wax Parti by Weight 61.4 15.0 6.4 Mix and heat the ingredients at 250 to 275 F until melted. Raise temperature to 300 to 325 F and add the following with agitation: Vinylite AYAA Ethyl Cellulose 12.9 4.3 Formula 16 Ingredient Nevlndene R-3 or Cumar W-l Santichcr 8 Rosin WW Vinylite XYHL Mineral Oil Paraffin Wax Parts by Weight 30 15 35 15 S 5 Formulas 17 through 19 are good suggested starting points for the development of hot melts for application between 160 and 180 C. By changing the type of polyvinyl acetate resin utilized In the hot melt, the viscosity of the melt can be increased or decreased without changing the ratio of resin to plasticizer, For example, substitution of Gelva V-15 for Gelva V-7 in formula -lions 17 and 18 increases the melt viscosity. '-Ingredient* Gelva polyvinyl acetate resin V-7 Ethyl cellulose Gelva C-SV-16R Santicizcr 160 Rosin WW Dibutyl phthalate Aroclor 1254 Formula 17 100 ' --- -- --` 75 ' 30 55 Paris by Weight Formula 18 65 15 '-- ` 16 -- 4 Formula 19 -- -- 100 -- 75 30 55 II Q222f>$l TOWOLDMON0027171 WATER_PCB-00011640 i Polyvinyl butyral hot-melt adhesives are useful for joining cellophane, aluminum foil, glassine, and waxed glassine to themselves. The sealing temperature is usually 200 to 350 F. The pressure can range between 0.5 psi and 30 psl, Polyvinyl butyral hot melts are extremely fast Ktling--usually from 0.5 to 2 seconds. The molten adhesive is usually applied to both surfaces to be bonded and allowed to cool and set. The surfaces are then brought together, and the bond Is formed under heat and pressure. Formula 20--Polyvinyl Butyral Hot-Melt Adhesive Ingredient! ' Butvar B-76 Opalwax Poly-pale Ester # 1 Staybelite Ester #10 Sonticlzer B-16 Armid HT Parts by Weight 10.5 30.5 19.7 14.7 6.0 11.0 The procedure used to make Formula 20 is to dissolve the Butvar B-76 in ethanol. The wax Is then added with agitation and slight heating until a homogeneous slurry is obtained. The alcohol is then distilled from the mixture, and the other ingredients are added to the molten Butvar-wax mix. To obtain a smooth formulation, the finished compound should be strained through two thicknesses of cheesecloth. Formula 21 is a polymethyl methacrylate hot-melt adhesive used to join cloth for inner liners, fabrics, or backings. Formula 21--Polymethyl Methacrylate Hot-Melt Adhesive . -Ingredient* Polymethyl methacrylate Sotitkker 160 Chlorinated rubber Parts by Weight 100 10 20 A typical cellulose acetate hot-melt adhesive is shown in Formula 22: Formula 22--Cellulose Acetate Hot-Melt Adhesive Ingredients Cellulose acetate Santtcher M-17 Inert filler Parts by Weight 50 8 35 12 0222552 \) o) TOWOLDMON0027172 WATER_PCB-00011641 I Cellulose acetate butyrate is commonly used for hot-melt applications. Formula 23 is a typical starting formula. Formula 25--Cellulose Acetate Butyrate Hot-Melt Adhesive Ingredients Half-second cellulose acetate butyrate Awclor 5460 Dioctyl phlhalate Newport V*40 Santonox* ynFleur#6 ' Farts by Weight 35.00 30.00 15.00 10.80 0.1 0.01 The above coating can be applied at about 350 F. Ventilation should be provided. A typical starting formulation for an ethyl cellulose hot-melt adhesive is shown In Formula 24. Formula 24--Ethyl Cellulose Hot-Melt Adhesive Ingredients # Ethyl cellulose, 50 cpr Lopof No. 45 Mineral Oil Bakers No. 15 Castor Oil Epoxy soybean oil Paraffin wax (m.p. 135 F) Santonox Aroclor 5460 Fart* by Weight 24 57 5 3 3 1 7 DELAYED-TACK ADHESIVES Delayed-tack adhesives differ from hot-melt adhesives, which become nontacky upon cooling. Delayed-tack adhesives are normally tack-free at ordinary temperatures, after they are spread and dried on a surface. After subsequent heat activation they maintain tackiness lor from sev eral hours to several days over a fairly wide temperature range. This slow-setting property per mits necessary mechanical handling before the adhesive cools and sets. Santonox: Monsanto Chemical Company trademark. Registered in U.S. Patent Office. I 13 0E2***3 I TOWOLDMON0027173 WATER_PCB-00011642 Solid plasticizers, such as diphenyl phthalate, Sotukizer 1-H, and Santicizer 9, make possible the delayed-tack properties of these unusual adhesives. The solid plasticizers are chosen for their compatibility with the base resin, their solvency action on the base resin, the tempera ture at which the adhesive is activated, their lack of disagreeable odor, and their crystallizing characteristics. I The patent literature relating to delayed-tack' adhesives should be investigated by those desir-[ Ing to produce them; for example, U. S. Patents 2,462,029; 2,608,542; 2,608,548; 2,615,156;! and 2,613,191. Formulas 25 through 27 are quoted from the patents as indicated. I Formula 25--Delayed-Tack Adhesive <U. S. Patent No. 2,462,029, Example 96) Ingredients Santicizer 1-H Vinsol Resin Thinned amine dispersant Acrysol M.R. Farts by Weight 50 50 250 10 "The thinned amine dispersant is a mixture composed of 1 part stearic acid, 1 part Poly-pale resin, a polymerized rosin containing approximately 40% dipolymers of abietic acid (Hercules Powder Co.), 1 part 2-amino*2-methyl-l-propanol (Commer cial Solvents Corp.), and 3 parts water. This composition is designed solely as a dispersion assistant.................." (from column 10 of this patent) Formula 26--Ddlayed-Tack Adhesive <U. S. Patent No. 2,462.029, Example 18) Ingredients Diphenyl phthalate Nevtndine R-3 Thinned amine dispersant (see formula 25) Hycar OR-25 ' Farts by Weight 52.5 30.0 198.0 43.5 The above formulation is non-tacky at ordinary temperatures and Is heat activated at about1 150F. The compound then remains adhesive through temperatures as low as 50 F. Once' set, the adhesive continues to hold at ordinary temperatures. I ') 02225^ | TOWOLDMON0027174 WATER_PCB-00011643 0 I l Formula 27--Polyrtyrene-Emultion, Deloyed-TacV Adhesive (U. S. Patent No. 2,615,156, Example 1) "1m llOi pans polystyrene (molecular weight 10,000 to 15,000) and 40 parts di|Arn>l phihalatr are mixed and heated together at approximately 190 F, forming a eirir lluid While still at this temperature, the fluid is poured into a solution oi a |urt of a 2S'r aqueous solution of Aerosol OT and 4.5 parts polyvinyl alcohol (of the grade sold under the trademark Elvanol 50-42) in 75.5 parts water; the K-lutMt heing at a temperature of approximately 190 F, constant agitation is main tained. mulling in a homogeneous emulsion. The emulsion is then permitted to mt" (This formulation is improved by the addition, after cooling, of 8 parts of flewi polyblcnd 550X70). This adhesive forms a smooth, non-grainy film when spread evenly on paper and dries to a completely tack-free surface. When heated to 170 F the film becomes sery tacky and powerfully adhesive. Formula 28--Polyamide Delayed-Tack Adhesive Ingredients Vcrsamid 940 joeliriser 9 Candcliila wax Isopropyl alcohol Toluene Paris by Weight 100 31.6 5.9 29.5 29.5 SOLUTION ADHESIVES Solution synthetic-resin adhesives differ from the emulsion adhesives in that solvents other than water carry the adhesive. The use of solution adhesives improves the "bite" or adhesion to many of the materials to be joined. Following Is a discussion of various solution adhesives. VINYL ADHESIVES - Formula 29 is a non-toxic, grease-resistant paper coating, which is readily heat sealable. Formula 29--Vinyl Solution Coating Ingradients Vinylite VYHH Vinylite VMCH Vinylite VAOH Scnlichcr 141 or Santicher M-17 Acetone Methyl ethyl ketone part, by Weight g0 10 J0 20 250 loo 02Z?^1 TOWOLDMON0027175 WATER_PCB-00011644 NITROCELLULOSE ADHESIVES Nitrocellulose-lacquer coatings are frequently applied to make cellophane heat scalable and mots*! ture resistant. Formulas 50 and 51 illustrate starting formulations for tbis type of application. Formula St Is typical of a starting formulation for a nitrocellulose cement. .I Formulas 30, 31, and 32--Nitrocellulose Lacquers and Cement Ingredients Nitrocellulose (#*sec.SS) Nitrocellulose (30-40 sec.RS) Dibutyl pbthal&te Djcyclobexyl phthalate Switcher 160 Santolite MHP Dammar wax Sanlolite MS-80% Paraffin wax Denatured alcohol Ethyl acetate Acetone Toluene Heat-Sealable Cellophane Lacquer Nitrocelluloie Cemont Parts by Weight Formula 30 Formula 31 Formula 32 15 -- 8 -- .-- 16 -- -- -- 15 51 '-- 15 50 -- 7 70 -- 12 8 -- 3 50 104 -- 50 -- 10 -- -- 5 -- -- 12 -- -- 34 34 -- CELLULOSIC ADHESIVES Formulations 53 and 34 illustrate suggested starting formulations for cellulose acetate butyrate. Formula 33--For Seating Paper to Paper or to Cellulose Acetate Butyrate Ingredients Parts by Weight Cellulose acetate butyrate (half second) Sanlolite MHP Ethyl alcohol (95%) Isobutyl acetate Toluene - Hi-Flash naphtha IS 15 15 10 35 10 It 0 0222 556 TOWOLDMON0027176 WATER_PCB-00011645 !* 1 If j ! i f i i .< 1 Formula 34--For Sealing Paper to Cellulose Acetate Ingredients Cellulose acetate butyrate (half second) SantolUe MHP ^ Ethyl alcohol (957c) Isobutyl acetate ' Toluene Hi-Flash naphtha Parts by Weight 12 18 IS 10 35 10 Formula 35 gives outstanding grease resistance and light stability. Formula 3$--Grease-Resistant Coating Ingredients Cellulose acetate LL-1 Sanlicizer M-17 Santicher 8 Acetone Methyl ethyl ketone Methyl cellosolve acetate thyl lactate Parts by Weight 20 10.2 25 16.8 - 37 7 7 A formulation useful for self adhesion of ethyl cellulose is as follows: Formula 36--For Self Adhesion of Ethyl Cellulose Ingredients fcthyl cellulose N-14 lewlso! 38 Dibutyl phthalate Toluene-alcohol blend (4:1) Parts by Weight . 10 5 1.5 83.5 17 `* 022?Sb? t6w`OLDMON00271 77 WATER_PCB-00011646 POLYURETHANE ADHESIVES . The advent of urethane foam has increased the need for adhesives to bond it to itself or to other materials. Formula 37 is an example of a good starting formulation for this application. Ingredients Multranil 176 Mondur C Ethyl acetate Arodor 1254 Formula 37---Polyurethane Adhesive Parts by Weight 100 s so 20 1 Formula 37 has a maximum work life of 48 hours. Excessive humidity or temperature shorten the work life. It is recommended that only enough adhesive for one day's use be mixed at a time. The formula may be diluted with acetone or ethyl acetate if desired. This adhesive may be applied by a cold method. The adhesive is applied, allowed to stand at room temperature for 10 to 30 minutes until the solvent evaporates. The pieces to be joined are compressed at 50 psi for at least 15 seconds. The adhesive surfaces may also be heated with infrared lamps to 130 F for 4 minutes to evap orate the solvent. While still warm, the pieces should be pressed together at 50 psi for 3 to 10 minutes. CHLORINATED-RUBBER ADHESIVES Chlorinated rubber is used in heat-sealing adhesives because of its low moisture-vapor transmis sion, chemical resistance, and heat sealability. Formula 38 is a suggested starting formulation for a heat-sealing chlorinated-rubber adhesive. When 5 to 7 pounds are applied to a ream of paper, this coating allows only 1/16 gram of moisture vapor to pass through 100 square inches of paper In 72 hours. Ingredients Parlon 125-centipolse type Aroclor 1254 Arodor 1260 Dibutyl phthalate Paraffin Wax Pentalyn H Toluene Solvent Formula 38 Heat-Seating Chlortneted-Rubber Adhesive Formula 39 Chlorinated-Rubber Label Adhesive Parts by Weight 60 -- --' ' 14 5 21 . as needed 20 6 6 -- -- -- 68 -- 18 ),*) O 0222*58 TOWOLDMON0027178 WATER_PCB-00011647 ZEIN ADHESIVES Formulations 40 and 41, based upon tern, illustrate the versatility of Monsanto plasticisers to produce specialty formulations with unusual characteristics. Formula 40--Zein label Varnish Ingredients Zein Rosin WW Sontolite MHP SQMkhtr 8 Proprietary or 91 % isopropanol Farts by Weight 100 100 20 25 190 Formula 41--Zein Foil-Tinting Ease Ingredients Zein A Sqntotite MHP Sartlicker 8 9l% Isopropanol 85% Phosphoric acid Coloring Parts by Weight 100 65 70 230 2.3 as needed PRESSURE-SENSITIVE ADHESIVES Pressure-sensitive adhesives are materials that are tacky at ordinary temperatures and require little or moderate pressure for fixing in place. Formulations 42 through 45 illustrate four pres sure-sensitive adhesives. Formula 42--Pressure-Sensitive Adhesive (calender onto fabric) Ingredients .. Cellulose acetate (type A-9, 40 mesh) Sanlichcr 8 ' Sontolite MHP Parts by Weight 1 2.5-5 1-2 t 19 0222559 TOWOLDMON0027179 WATER_PCB-00011648 Formula 43---Pressure-Sensitive Adhesive (calender onto fabric) Ingredients Vinylite AYAF (polyvinyl acetate) Arofene 700 (100% phenolic resin) Sontkieer B-16 ' Parti by Weight 5 36 IS Formula 44--Pressure-Sensitive Adhesive (hot-melt type) Ingredients Pale crepe rubber Vlstanex (polyisobutylene) Ester gum Santolite MHP Methyl abietate, Sonticizer 160, dibutyl phthalate, Aroetor, or Sonticizer B-16 Wax (Montan, paraffin, camauba, or amorphous microcrystalline) Perk by Weight 15-20 5-15 20 20 25-50 1-20 Melt all components except rubber at about 210 F. Add rubber, and reduce temperature lo 180 F. Stir at this temperature for 1 to 2 hours until mixture becomes smooth. Hot cast on suitable surface. . -Formula 45--Pressure-Sensitive Adhesive (solution type) Ingredients Farlon 1259 type Staybelite Ester # 10 Pibutyl phthalate Acetone Hexane Pertt by Weight 5 ' 10 10 52.5 22.5 0 0 0 0222560 | TOWOLDMON0027180 WATER_PCB-00011649 'i ADHESIVE PRIMERS Adhesive primers are used in the same fashion as paint primers; that is, one is applied as a preliminary coating so that the secondary coating cjin adhere better. The secondary coat may be any type of vinyl chloride, if thj primer, such as the one illustrated in Formula 46, is first applied. Formula 46--Adhesive Primer (for bonding vinyl to paper or cotton doth] Ingredients Vinylite VYMS Vinylite VMCH Santidzer 160 Methyl ethyl ketone Solvesso No. 1 Parts by Weight n 2 1$ 25 17 Since synthetic fabrics, such as nylon or Dacron, have particularly non-adhesive surfaces, ad hesive primers are especially useful. Formula 47 provides a very effective adhesive primer coat for nylon and Dacron, as well as for metal. Formula 47--Adhesive Primer for Synthetic Fabrics Ingredients Vinylite VMCH Vinyl Resin Dioctyl phthalate (DOP) Methyl ethyl ketone Mondur M Parts by Weight ' 100 60 200 5 Formula 47 is made by mixing methyl ethyl ketone with the plasticizer, then adding the resin. The shell life of the mixture is indefinite until the Mondur M is added. Upon addition of Mondur M the adhesivity of the compound decreases by 15 to 20 percent in 10 days. Accord ingly, Mondur M is added last, just before the adhesive is to be applied; and only as much ad hesive should be finally compounded as can be used within a day or so. 21 TOWOLDMON0027181 WATER_PCB-00011650 r MISCELLANEOUS FORMULATIONS 0 EPOXY-RESIN ADHESIVES _ ' Epoxy resins are widely used in adhesive applications. Monsanto Chemical Company's Mod- JEpox* organophosphorus compound improves the bond strength of epoxy adhesives (Formulas 48, 49, and SO). Mod-Epox also reduces the viscosity of epox adhesives, maintains chemical resistance, and lowers the cost considerably. I Formulas 48, 49, and 50 -- Epoxy-Retin Adhesives Ingredients Liquid epoxy resin (EV-200) Diethylenetrlamine Mod-Epox Butyt gtyctdyl ether Formula 48 Formula 49 Formula 50 Parts by Weight 100 100 100 12 . 8 - 25 13 -* -- -- 13.5 Cure: 20 hours at room temperature plus 2 hours at 100 C. Tensile Sheer-bond Strength Aluminum - Aluminum Steel Steel Class - Glass >Ooheslve failure of resin. Adhesive bond intact. Formula 48 1880 psl 2000 27S0 Formula 49 2590 psi 3060 4900* Formula 50 2010 psi -- -- Aroclor and JlSenior* chlorinated polyphenyls are frequently used to extend epoxy adhesives and coatings. The use of these materials greatly reduces costs with a minimum effect on chem ical resistance or adhesive characteristics of the compounds. Mod'Bpox; Mentor; Monsanto Chemical Company trademarks. Registered in U. 8. Patent Office. 22 0 Q OZiiibi I TOWOLDMON0027182 WATER_PCB-00011651 c POLYURETHANE-RESIN ADHESIVES Polyurethane resins are commonly used in flocking adhesives. The following formulation is typi cal of a flocking adhesive: ' Formula 51---Polyurethane-Resin Flocking Adhesive Ingredients Part A -- Multranil I LD Aroclor 1254 Mondur C Part B -- Multranil KLD Mondur C Parts by Weight 100 20 5 100 5*10 Part A Is applied to the fabric by knife coating and allowed to dry thoroughly. The fabric is then coated with Part B, and the material is flocked immediately. TOXICOLOGICAL CHARACTERISTICS 5 The 1058 amendment to the Pure Food, Drug, and Cosmetics Act has caused some uncertainty about the kinds of materials that can be used in adhesives. The Food and Drug Administration has ruled that it will approve any material that does not migrate from the adhesive into the food. Migration is determined by use of a suitable dye. Monsanto offers six plasticizers that are approved by the Food and Drug Administration as being non-toxic. These products are: , Sonticizer 141 5<mficfeer B-16 ' . Sonticher E-15 Diethyl phthalate .... VDioctyl phthalate \' (For foods with high water content only) Diisooctyl phthalate j Use or these materials as plasticizers in synthetic adhesives should greatly aid acceptance of the adhesive. 0222*63 | TOWOLDMON0027183 WATER_PCB-00011652 i INGREDIENT INDEX Ingredient Identification Supplier Acrysol* Aluminum oxide Ammonium caseinate ' Armld* Arofcne* Bakers castor oil . Butvar* Butyl glyddyl ether Candelilla wax Carboxymethylcellulose Cellulose acetate Cellulose acetate butyrate Chlorinated rubber Cumar* Dammar wax Diethylenetrlamlne Elvacet* Epoxy soybean oil Ester gum Ethyl cellulose Gelvft* Ceon* Hycar4 Eewlsol* Lopot* No. 45 Methyl abietate Synthetic-resin emulsions Amides Modified phenolic and maleic resins Polyvinyl butyral resins Coumarone-indene resins Polyvinyl acetate emulsion Polyvinyl acetate emulsion Polyvinyl materials Resins and synthetic rubber products . Rosin-modified maleates Mineral oil , Rohm & Haas Co. ' Reynolds Metal Co. National Casein Co. Armour Industrial Chemical Co. D. S. Industrial Chemicals, Inc. Baker Castor Oil Co. Shawinigan Resins Corp. Shell Chemical Co. Concord Chemical Co. Antara Chemicals Division General Aniline fit Film Corp. Eastman Chemical Products Co. Eastman Chemical Products Co. Hercules Powder Co. Allied Chemical Corp. Hathaway Allied Products Union. Carbide Chemical Co. E. I. du Pont de Nemours & Co. Rohm Si Haas Co. Glidden Company Hercules Powder Co. Shawinigan Resins Corp. B. F. Goodrich Chemical Co. B. P. Goodrich Chemical Co. Hercules Powder Co. Esso Standard Oil Co. Hercules Powder Co. Trdmrk rccfcter<d in U.S. Patent Oltice. 24 0222564 0 TOWOLDMON0027184 WATER PCB-00011653 Ingredient Index Continued Ingredient Identification Supplier Methyl Cellosolvc* acetate Union Carbide Chemical Co. Mondur* Isocyanates # Mobay Chemical Co. Montan wax - Beacon Company Multranil* Synthetic resin Mobay Chemical Co. Nevlllac* Nevindene* Phenol-modified coumaroneindene resins Coumarone-indene resins Neville Chemical Co. Neville Chemical Co. Newport V-40* Pine resin Newport Industries, Inc, Nitrocellulose Hercules Powder Co. Opahvax* Parlon* Pcntalyn* Foly-G* P-1200 Castor oil, synthetic wax Chlorinated rubber Penlaerythritol esters of rosin Polypropylene glycol Baker Castor Oil Co. Hercules Powder Co. Hercules Powder Co. Olin Matheieson Chemical Co. Poly-pale* esters Polyco* Glyceryl & glycol esters of polymerised rosin Polyvinyl acetate emulsion Hercules Powder Co. The Borden Co. Polymethyl methacrylate Rohm & Haas Co. Polyvinylpyrollidone Quflon* Solvesso* Chrome complex Aromatic solvent Antara Chemicals Division General Aniline & Film Corp. E. I. du Pont de Nemours & Co. Esso Standard Oil Co. Staybelite* esters Hydrogenated rosin esters Hercules Powder Co. Syri Fleur* Odorant Syn Fleur Scientific Co, Triton* X-1SS Versamid* Vinsol* . Wetting, emulsifying, dis persing, scouring agents Polyamide resins Pine resin Rohm & Haas Co. General Mills, Inc. Hercules Powder Co. Vinylite* Vislanex* Vinyl resins Polyisobutylene resin . Union Carbide Plastics Co. Enjay Company York Whiting* Superfine calcium carbonate National Gypsum Co. 2ln . Corn Products Sales Co. Trademark reentered In U.S. Patent Office. 02*2565 I TOWOLDMON0027185 WATER_PCB-00011654 TECHNICAL LITERATURE ABOUT MONSANTO PLASTICIZERS Tbc following technical bulletins and brochures give technical information about the properties and applications of the Monsanto plasticizers and other products that are mentioned In this bulletin. Monsanto technical literature is continuously revised to contain the most recent and reliable information possible. Your request for any literature will be promptly and cheerfully filled--without obligation, ol course. N General "Monsanto Plasticizers"; Booklet containing technical data about all of Monsanto's plas ticizers "Seven Plasticizers for non-toxic applications" "How you can benefit from Monsanto Solid Plasticizers" Phllialate Plasticizers Santicher 160 (butyl benzyl pbthalate): Dibutyl Pbthalate: Diethyl Pbthalate and Dimethyl Phthalate: Dicyclohexyl Phthalate: Di-(2-ethylhexyl) Phthalate (DOP): . Diphenyl Phthalate: Technical Bulletin PL-160 Technical Bulletin PL-302 Technical Bulletin PD303 Technical Bulletin PL-312 Technical Bulletin PL-318 Technical Bulletin PL-319 Phthalyl Glycollate Plasticizers - Santicher E-15 (Ethyl phthalyl ethyl glycollate): . Santicher B-16 (Butyl phthalyl butyl glycollate): Santidzer M-17 (Methyl phthalyl ethyl glycollate): Technical Bulletin PL-15 Technical Bulletin PL-16 Technical Bulletin PL-17 Phosphate Plasticizers Scnlidser MO: Santicher 141 (non-toxic plasticizer): Triphenyl Phosphate (flame-retarding plasticizer): Trlcresyl Phosphate(flame-retarding plasticizer): Technical Bulletin PL-140 Technical Bulletin PL-141 Technical Bulletin PL-301 Technical Bulletin PL-305 26 0 e 0^^^ibb | TOWOLDMON0027186 WATER_PCB-00011655 Sulfonamide Plasticizers Scnlicfzf-r 1*H: Sonticizer 8: Scnticizcr 9: Technical Bulletin PL*1-H Technical Bulletin PL-8 Technical Bulletin PL-9 Arodor Plasticizers The Aroclors: Application Data Bulletin O-P-115 Arocbrs 1221, 1252, and 1242 for polyvinyl acetate emulsion adhesives: Technical Bulletin PL-321 Other Plasticizers HB-40 (partially hydrogenated terphenyl): Mod-Epox (epoxy-resin modifier): Resin Additives SaHtolite MHP and Santolite MS-80/r (Monsanto industrial resins): Technical Bulletin 0*104 Technical Bulletin PL-313 Technical Bulletin PL-320 Preservatives and Stabilizers Santobrite and Penta for the preservation of paints and water-ba* adhesives: Santouox and Sontoitox R, antioxidants for polyethylene; Sodium Benzoate, Technical: Technical Bulletin SC-2 Technical Bulletin PL-324 Technical Data Sheet Odor-Masting Agents "Coumarin Monsanto": "Methyl Salicylate Monsanto": . Santomask 11, Odor-Control Agent for Paint, Ink, Plastics, and Other Odorous Products: "Vanillin Monsanto": folder folder Technical Bulletin PL-325 folder 27 TOWOLDMON0027187 WATER_PCB-00011656 SHIPPING INFORMATION I Most Monsanto plasticizers are shipped in bulk in tank cars or tank trucks (within estab lished delivery zones) from six strategically-located bulk-storage stations. As supplier of the world's largest selection of plasticizers, Monsanto offers savings through mixed shipments of different plasticizers (compartmented tank cars and tank trucks or mixed trucklots of drums) for all of your plasticizer needs. Mo shipping limitations apply to any of Monsanto's plasticizers. Shipping classifications and bet contents of standard containers are tabulated below for the plasticizers mentioned in this bulletin. Standard Containers Preduet Qasstfieation 55-gal. drums (lb., net) 5-gel. drums (lb., net) Dimethyl phthalate Diethyl phthalate Dibutyi phthalate Dioctyl phthalate Dicyclohexyl phthalate Diphenyl phthalate Switcher 160 Switcher E-15 Sanlicher B-16 Santicher M-17 Dimethyl phthalate Diethyl phthalate Dibutyi phthalate Dioctyl phthalate Dicyclohexyl phthalate Diphenyl phthalate Butyl benzyl phthalate (Resin plasticizer) Resin plasticizer Resin plasticizer Resin plasticizer 530 500 475 445 350 400 500 535 500 550 40 45 40 40 -- -- 40 45 40 SO Trlcresyl phosphate Triphenyl phosphate Switcher 140 Switcher 141 Switcher 1-H Resin plasticizer Resin plasticizer Resin plasticizer Resin plasticizer Resin plasticizer 530 45 225 -- 545 50 495 45 -- 80" Aroclor 1121 Arcelor 1232 Aroclor 1242, 1248, 1254, 1260 Aroclor 5460 Synthetic resin Synthetic resin Synthetic resins Synthetic resin , 520 550 600 500 ___ -- -- --. HB-40 Moi-Epox Sonlolile MHP Stmlolile MS-80% Sanlomask II Sontonox Resin plasticizer Chemical, NOIBN j rail; synthetic resin ' \ without filler / ] truck: synthetic resin, / solid mass | Chemical, NOIBN Chemical, NOIBN it 450 40 510 45 -- 60(b 540 45 250" ISO 45 -- fcortugated carton (16'* x 8" * 9") >7 gallon *>)) gallon t 68 2-2931-0969-6 lltHO IN U.S.A I TOWOLDMON0027188 WATER_PCB-00011657 AKRON ATLANTA S0510N " CHICAGO , CINCINNATI t DETROIT ! HONOLULU ) HOUSTON | LOS ANGELES I NEW YORK I ST. LOUIS ([ SANTA CLARA | SEATTLE I SPRINGFIELD | WILMINGTON Monsanto MONSANTO COMPANY ORGANIC CHEMICALS DIVISION 600 NORTH LINDBERGH BlVD. ST, LOUIS, MISSOURI 6SI6S o 23000. ZSBSHK:.' 0222*^ TOWOLDMON0027189 WATER_PCB-00011658