Document zQBakeXdO1n04kz075BG0x0ez
&
m4
X>ate.
MEMORANDUM
SHREVEPORT
c< i Mi l"-?ulwefco -Hr* PotSaw--
7-16-55 pmrn B*P.Soward T,, Mr. Chamberlain
- Etf
I am enclosing report written by Dick Potter covering the trial runof dry felt using the auxiliary spray on MasterbiIts for the first and
second shift and then running the companion rolls of dry felt on both shifts the following day with the auxiliary spray off*
It is important to note that we were unable to obtain proper saturation
with ths auxiliary spray off and, too, we were unable to run over 150 volts or 270 feet per minute* Whereas with the auxiliary on we ran between 225
and 240 volts, or 405 to 432 feet per minute* This, is a tremendous
difference in speed and also at the 405 to 432 feet per minute with the auxiliary on we obtained much better saturations*
In order that ths test be as fair and accurate as possible, I spent a good deal of time on the machine with Potter* He was there continuously
during the test so that accurate information oould be given you* Both Potter and I feel as theugi this is as fair a test as we could run*
It seems whan the sheet is properly doctored at the saturator to dry sufficiently at the coater that much of the saturation is removed from the Aset* The auxiliary allows the excess saturation to strike in and then be re-seraped by allowing nhot stuff" to cover the surface of the
sheet*
W Xn your memo of 7*6*55 you asked for further comments regarding asphalt used in the month of May* We are not satisfied with the average percent
. saturation on 15 pound or 30 pound saturated felt. As a matter of fact, we have difficulty obtaining I4O5C saturation. We do feel that if we were able to apply a totter saturation material at the auxiliary spray that we could use It on 15# felt and do'an excellent job* We might, however, need doctor blades on the balance of our bottom strike-in rolls to dry the
edges*
At the present time we are not using the auxiliary spray on 15# and 30# fslt because of mmtndgee* We also fsel that a hotter application of saturation at ths auxiliary spray would help on heavier weigit dry fslt
for ell products*
To us this test indicates that on 15# and 30# felt we are actually doctoring the saturation from the sheet in order to properly dry it*
It also indicates t hat when we are not using the auxiliary that we do not substantially Increase percent saturation by slewing down the machine.
We have had reports of this from our machine men running 15# and 30# felt* We i*ve also checked with them many times to substantiate their statements.
During May our actual vs standard was as follows:
111.92 tons under on saturation
C) tons tinder on coating
tons under on asphalt saturation A coating
264.62 tons over on filler
TEE tons over on asphalt saturation, coating and
filler
------- ------
Also as mentioned in my memo of 5-27*55:
BIRD 014175
f fe NM
MEMORANDUM
SHREVEPORT
fa Reply toDateFromTo.
"As to the actual vs standard - I do not believe the individual items of saturation and coating used to standard can be analysed properly unless the filler is taken into consideration* What we do at Shreveport is to figure as follcers:
The Accounting Department takes the amount of saturation used per standard and the amount of coating used per standard* These two axe totalled and the percent of the total of saturation and coating is figured. This percent is then used to break down the amount of actual saturation and amount of actual coating used from the asphalt department after actual Inventories are taken and total actual aaphalt used is determined* Therefore, the more actual filler used the less asphalt would be used in proportion*
"We have constantly for the last ten years talked and preached using the proper amount of filler, as it seems very easy to not use what is necessary*"
In addition to this the accounting ahows asphalt flux and saturation as one total received asphalt figure each month and sheers on all asphalt a 4% shrink due to blowing loss* However, about 60% of the saturation used ^ is purchased as straight saturation and already blown* Therefore, there Hjp would be no shrink to be deducted* At the present time about 25% of all asphalt purchased is straight saturation* This would indrease the saturation use some*
BPS:lb
BIRD 014176
ion (fc`B4 Dta:<3
In Reply to.
MEMORANDUM
SHREVEPORT
n.t.7/18/55
Fmm PSL-Potter
TnMr. Chamberlain - B.W.
Subject.
FS SATURATION WITH AUXILIARY SPRAY OR ARP OFF
,,ie following report la on the run3 of companion rolls of 50x48 dry felt from the same reels run on FSPM-1 on 7/12/55 and 7/13/55* All rolls run on 7/12/55 were saturated with all sprays on In the saturator and run out of the saturator wet Into the auxiliary spray, which vas on, then scraped so that the sheet was dry or slightly mottled Into the coating rolls. All rolls run on 7/13/55 were comjwanion rolls of those run 7/12/55* Bu this
case the rolls were saturated with all sprays on In the saturator and run out of the saturator as wet as could be and still be approximately as dry
Into the coater rolls as the rolls run 7/12/55* Neither the auxiliary spray nor the auxiliary scraper was used on these latter rolls.
It was originally planned to run the rolls used on 7/13/55 as fast as the ones run on 7/12/55. However, It was found that we could not run this fast since the material would not saturate at the speeds that were run on 7/12/55* As a result we started each roll on 7/13/55 into the machine at 150 volts or approximately 270 feet a minute. After obtaining a saturated sample at this speed we would increase the machine speed to 200 volts or approx. 550 feet a minute for 2% minutes, take another saturated sample, and then revert back to the 150 volt speed. In all rollB but 3 we found 3mall l/32 - l/l6dK spots of unsaturated felt at the 200 volt speed so did not attempt to run any higher for samples. It was necessary to hold at this speed for 2\ minutes to allow time for the sample to go all the way thru the saturator and strike-in
section before getting samples.
tried running the machine both days so that we would get at least the Ifl^inimum % saturation of 165# on machine checks. In the case of the 7/12/55 run
'"there were two rolls, run on the nlte shift, where we had to slow down and take additional samples to get this 165# saturation. In both cases we
maintained this lower speed for the balance of the roll.
In the case of the 7/13/55 bun we had to take as many a3 3 samples and even then were not too successful in obtaining 165$ minimum samples.
After the two runs extractions were taken on all samples and % saturations
were computed. The following figures are compiled to show companion rolls
and the resulting # saturations. The attached work sheet shows this same
data, plus roll kerosenes, PSL kerosenes on extracted samples, machine
saturations, PSL saturations by extraction, and machine speeds,
DSPM-1 i> Sat ./y Sat^t DSPM-1
Condition
Condition of
Date
HxtrrAux Ext rA.ux. Date
of Sheet
sheet into coater
Bottled Mottled
Tour Roll On
3/7/7/55 180" 24 C __ 3/7/7755 17*T
Off i3?r
t-,138"
Tour R1
Into _C--oater
77/7/55 fc-dry, S-6 1 -9"Vet
:4 A __ !______
__ .
straak
3/7/7/551 R-dby73-2"^31,~wet
Mottled
25 B. 3/7/7/55 165
' 133
25 A
'
streak
3/7/7/55;N-dry,S-6n-9ff wet strea
__________ _ L 26. B.
26A____ L____
....------------------
Slightly mottled
; 3/7/7/55
q
i
177
Mottled '
: 3/7/7/55 ' 187
160 160
3/7/7/55'N-dry-S-3
wet strea
27 EL... 1
. . -tt-- _
3/7/7/55iH-dry-S-2 -3 wet strea
^ ; 28 0 Hi^iightly mottled 3/7/7/55 191
'157
18 B .. I .............
__
/777/55 lN-dry-S-^ wet strea
____ Mottled
...30 B 1/7/8/55 167
144
"^/55 N-dryjS-^j-^ wet strea
.5 c
;
|5.A.__ .
BIRD 014177
r
IO .*,-114 OIBT#
MEMORANDUM
SHREVEPORT
la Reply to-------------------------------------- DateFromTo.
TSPH^I------ $ sat,
$
"TSFH^I
Condition of
Bate
ExtrrAux. ExtrrAux. Bate
sheet Into coater Tour HI. On
Off Tour RIj
condition of Sheet Into Coater
Slightly mottled 1/7/8/55 169 6B
Slightly mottled 1/7/8/55 181 -8 C . ,
Slightly mottled 2/7/8/55 182 21 B
Slightly mottled 3/7/8/55 161 25 A
Mottled
377/8/55 178 26 B
Slightly mottled 3/7/8/55 193 27 C
Mottled
3/7/8/55 186
28 C ,
Mottled
I/7/9/55 171 1B
Slightly mottled 1/7/10/55 178
J10_______
140 132 T55 137 141 133 139 139 151
1/7/8/55 H-dry,S-l2"-15" wet
6 A streak
1/7/8/55 H-dry,S-6
wet
8 A streak
2/7/8/55 N-dry,S-6 -7 wet streal
21 A
3/7/8/55 H-dry,S-2" wet streak
25 C
3/7/8/55 Bry
26 G
3/7/8/55 N-dry,S-9n-12" wet
27 A
___________
streak
3/7/8/55 N-dry,S-6" wet streak
28 A
1/7/9/55 IT-dry, S-3" wet streak 1c
1/7/10/55 ,N-dry,S-6M wet streak ______
In describing the condition of the sheet Into the coater It was possible when |gj||tng the auxiliary scraper to control the condition of the sheet from a ISightly mottled sheet - approx. 5$ of sheet with small spots of surface saturation to a. mottled sheet - approx. 10$ of sheet with small spots of
saturation. On 7/13/55 where we were not using the auxiliary spray or scraper we had more difficulty drying the sheet and therefore almost the entire rim had a streak on the far south side of the sheet which was wet Into the coater. All samples were taken from the north (aisle) side of the sheet and no sample, from eljbher day, had any excess saturation on it. In addition all mottling and streaking was on the top surface of the sheet with none on the back.
HKP/gf
i
J
BIRD 014178
V ^ *w
5 0o3'
Si;
NVM n ^ ft ^
* 0 ft 0 o <1 n *> fft fft
l v v "2 v X <*
*3 N \ N
^
* X
* *>
ft ft. \\
<S. +
ft> * XX
;*
^^ ^X
* v *> u *
v* x o % x *V X Xm x-xN
4> *v
as
w
K
<N
IN
* X ft n> > ft
X *1
X
X
Nx
X
O9 9 O o
18 tii
S i U ! U$
| ? f o S V v* >>> >
> ti V
s \
V#
X
^
X
* X X ^ VH < x xNx
> \i 9 "
X v X "3 .0 V ^
N v* X* xx \V :l\ <*s
%
03
be*
iiv 0 ^
'M *
o0 -nP *H
v;
oo^ft
Q * ft
II
51
X ^ v V~ ^U Vs#ts.f4 ^ ^ 'J \l ^
KS>-
1 *> ft <1 nj (>j ft> ftr ft
r>
rt
I o 0 C* X5 fX x rl H \ ^
X \, \** * ,' O * Q > X x * X 4
bi
co
I
J <4
* f-
H X
fT)
ft,
> X
ft ft
w X
4
x
4; x ts . <>,ft o c\ <X
XXX x
x V sS
II ^ ft N
v> \) (s 00 x n M <3 0
V V
H4W
'ftr H < rj "i
n 1
| ^ tt *1 * A & & s
n <ft fft
*> f> n
r>
'a
lo
jo
4
is*.i
Vf -fe.
u Vi v y ' ^^
gA^ngggnn^
iO
A
t
BIRD 014179
BIRD 0141?