AROCLOR PLASTICIZERS
A MriM of inert, chemiestiy-resistam, fire-feterding pitttictuK* compatible with wide variety of raeins.
tlCNNKAl UUJETIN O/PL-306A
Monsanto
0<t76G32
TOWOLDMON0033002
i
AiOCLOr PLASTICIZERS
A series of in&rt, cbermceify-resistam, tm-wWding ptmUmms compatible with wide variety of resins. TECHNlCAl UUTW O/S*L~30$A
?
ICIW. *.-> :.w, .i-.>
TsMucuy ftd #<*#
Handling, and environmental Hexzsrrfs, <m p**?* 12.
Oft*** tommk m&Kfm tt,
M. ; St law*.. ttteftmi #318 0476033
TOWOLDMON0033003
The unique Am&m* plasticisers are among the mast versatile chemi cally produced Materials available. One ouiatanding characteristic -- marttutt -- makes Aroclor useful In nutty ways for many different application*. He major benefits offered by Arocter include;
Chemical Resistance Rm Retardanee
Compatibility with most resins Manaxid&tion Adherivity
Lew Cost
Monsanto's Aroclor plasticizers comprise a series of chlorinated Mphmyte and chlorinated polyphenyls. They vary from mobile, oily liquids to white crystals and hard, transparent resms.
Twelve of the Aroclor plasticisers, each of which represents a series, ant discussed in this bulletin. An understanding of the system for designation of each Aroclor should prove useful in the evaluation of the property gyadations among them. The last two digits indicate the approximate weight percentage of chlorine in the product, and the first two digit* indicate the type of material, as follows;
12 -- chlorinated biphenyls
25 -- blend of chlorinated biphenyu, and chlorinated triphenyls
mm
44 -- blend of chlorinated bipheny's and chlorinated triphenyls (0,-40) *
54 -- chlorinated triphenyi*
Por nearly every Aroclor mer tinned a Ja.ker, lofo oore grade exists,
.#& . bout the ut.'U- deal r.nd
sharacteratits, but lower
: era.*.
_
________
____
The Aroclor liquids and resins arc readily soluble in most common organic solvents and drying oils. Although all Aroclor plasticisers are Insoluble In water, t&u imro, rrystaliric r.uterials are generally less soluble than the liquids and softer resins. Solubilities of some Aroclor plasticisers are shown in Table 1.
Qi, 76034
TOWOLDMON0033004
m-,t <
. *c'm
U%h Amu
_ -*n r* M>&
sctwunti m m&mmsfmmmvmmmmm
mchiim
*'*
Auvckttm
trt Km
And* lift
ire m
Anck'im
cm m
t. . 5!
%
..
--
$
s
s s
--
n * __ -
lf
--------
4V. 'Je
k
_ ..
^ htr.nm
.11111t1
vs vs v$ vs " vs ss ss
$ $ - -- s .s -- --
4*s
--
S"
--
--
,>, .ItMiMS - HWJ#V % S * s s s s --
. i 'Ufdl,.-<(
?
$
%
$
s
s
----
SMuuimm L: (IW
.s..
s --
% ~~
$ --
s
--
s
--
s
--
% --
l-k- ; -/,# 4(,,n>+ j s s s s s s s
$m-*> .t* - a{|n/p <*4
-4-
v
$
s
s
s--
> c.l #
-----------
Hi. n5*)rtU^e
......
TritWattthjflMt
s s s s $ * -- $ s $ $ $ s -- ~~ $ s1 $ s $ -- --
ft rat; M T wt 3ii l. ,d Os!
s s s $ s s -s s $ . &' s s I s
**
___ A*t' tow#
Ssssssss
iitirl $ ..... s $ $ $ s s s
.. "tdbsdw"' Actum ~J-- s s $ s s -- --
.........&*m%ni M ___ a;*wtoW#se
$ % s T" s % -- *-
sss$$$ss
Arnckr 44SS
cm mt
ss s s vs
----
AnctoSM
ire
--
1I
vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs s vs s vs
--
--
w -- -- -- ~~ ' -- -- ~~ ~~
--
--
-- -- -'
TOWOLDMON0033005
__
' $ ' ~S
r~ ' s'
____ tr.. i
3$
Ss4
___ ~
__ _______ * s s 1 s 4
_ 1 '>." Gln<0i*C4MM s'"
J"
s
s
. mm AotMt
ss s 4 4
ftlOMft Hw|IHII f 4 s 4 4
Eflw>. SlMtltar
S$ s 44
s -* 4 SS
4 ..... 1....
4--
4 "" ss S-- 44
kKimt
_...... twW
tt**
____ J*4m*/*___ _____ *
7* *
vs
VS 03fs !SS*rc
t
s 4 4 ' 'if....
ft, !!!..*
Hr U 3?!'` :f
-- ss
-- ss
"''pr'f""'
-- 30S@3*S
--
_..... )/S
vs vs vs w 4
__ few*_
V4
VS
VS ... vs "
vs
vs
w
K(mc.
vs "W vs vs vs vs SS
7 !<>{& '" " vs"vs"
n
vs
vs
vs
s
~ ?itmH " '
?.e}f ' "% ~ ~
s--4--
_ r'r-"
s
s'" n
vs
s
4
s
____ VS
ffs 'vs
vs vs VS
4
t' '
Vs"" "vs"
vs
vs
vs
VS ' S
. ***
vf vs vs vs vs , vs
4
,**H*8$
- 4 s $S
_ t bt-
!
S $, ' ~~
s4 1
_ t> 4 :! {3-A;
ilS*'*1.
--
28*
1
mu.,; fikssoi __ . !) ss% _ {*. A.tf'.e
** .swt .. .... tpvv
g
* ggjifre
$ s
* --
j11 -- tSc m
-- ss s
44
i -- SS I
.. ""I.......
m$ $ " VS ~~ VS ss 4
SS $4
VS VS VS vs 4 4
4 SS S4 --. 4 -- SS
-- -- --
4 VS VS -- vs VS 4 vs vs 4 m vs --u4 4s$ 4 vs m 4 vs vs 4 4 v$
Ss4
SS ss
4
I ss -
II
-- ss --
44S
i 44
w -- --
-- --
-- -- --
MS -- -- --
-- , 142
-- 128
-- --
-- -- -- 244
__ Cms** 2*rjfMe _ H'Uctr, *{Mi
$
s S 4 4 VS VS
$ -- -- 4 $ -- -- VS
--
_. *<
iitfitiiii~
1- iv An :s Sii|k% StteMt
VS -- Vwy SdnM,
*/ - -gw t.'im si Mm pr Mt sMUttm *f tglwM M 2S*C *) gHwwiw Miali,
,
9C09m
TOWOLDMON0033006
VMt
'
mMm.mmmM.mn.mmm mmmmrm
fmmi
Atfim&fffl Artamc/ar &mmkt(
tm
4flNMN*
fflohif* wi 8*0m88,*08 nUmM. si 8m*omijil,s oil
Attmt$6t?
{
w{
nmmtk nmmm '1MMPHA '109ATHA *188M>HA
Mam. pmetM
, 20J4-1J
Jk&titf, reax^ssm
*M14
mum*. w, mrimm
-
lias it9mttkiWlH *v#fC#Xj*fQ**l*S&tQ*f*i, *M*f$Z*G*!f*?u HHtTt {ti*48*Q
$m&fc Stimtf
*1.182*1.111
plffittfa ptf * ButitMml&m, % tmmitS
8.85
m-m
m-m %.m 8p.0r9-8is73re}
wnux> 1M8 m-m
42
*6.818 *8* 8J888* pr-85X) *1,3*1-13*2 <28718.8X1 11. 328-39*
48
*8.818
*58 8.88878
(2I*4RX) {*81S.47018S-1J.4X1}8
12.84 348478
84
*8.81#
*80
8P80`041r$ei *1.488-1485 (*/lUt>
12,82 365-330
fnpm*tmlms,% jTte M, *.}
11I038XX.,
$1um*i*
18-1.8
^7^{cttnMec*), xf\* muu-mm
fm trnm fltv*tod 0?8 &$}. j 57$ fj ^0
>** (ASTM1 ffl,
x! { >j
m*mg film {ASTH -28}, XX -
M*ej 1417-141S
ife s*fr SiEsa^i Sa^'57 0wt**l i
(ASTM U-tt)
106*8 139*8
|(3874..4rW`C)i|
*3841 3547
------_--- ----21-8-*-8-#--8.8-X--11j ,,,.3,,-6--3-1------
1 8-1.8 m-m
36^410
2M31B --3i1l5
83-.88-,438 175-1
344-384
j !hm m ` ,*r'1364! i ~U j2
1.828-1,822 | 1.127*1.121
u-r, K41
31-42
)
<X82-K-
3448
8149.-34.0 IB-1
378-384
Hkami!e*gtomnt
7 18.4
-
91.41-111 Nmmk
Nsmis
18 86
-
1.136-1.121
1.838-1.841
185-240
m*73u-40
21*4M840*-84341480M
0476037
TOWOLDMON0033007
Amkt tm
rtskyrMW
1MAPHA
m *4sm4 *56 W
prioro
i5551.UI (#1154*0 1156 j 311-428
' 611 ; M4.i ! D*l* f.............. j 8es* is ; Mi) trim
P m
_
1.BW.W
Amkt tm
UgH(*lsw min
Jfmstsf tm
150 Witt 61.5415
*6 SPA (fBSttsn)
42
Jwsfer m
now
2 MM (--Itw> 65
Amdm m$
Atmfor tm
Amt m
Block. opqu. fcrittlo fooio
Boot, ytttowt8-**5*f. MM* MM or fiokH
_ , *2 DBA
(BOto#!
Whit.tt off-whit* jHMnitr
*1.1 MPA (molttfi)
61
53.6-60.6
66
1616
6.05
641
1.4
0,05 0.05
-
0 08064 or-wti
-
6.66126 (21*4619
-
646661 (25*41*0
-
8.00g8 (8*46*0
~
14*17* (2l*-t24"C)
-
0 00087 (26*-186*0
*1.576.1.5*3 (667164*0
1.478 iwmm
1476 (2I*/25*C)
1.734 126721*0
1.678 (2572519
1494.1.611 (a*/a*c>
15.72 388425
#6.1 B.S44 Mon*t boiltag jisitil
1124
16.61
216-368 ( *.#)
236-32* (4 *.}
#41 *402 12 8.24.3
247 477
tsjjg'g-J.
1444
_
8.2-BJ
13.81 280-335 (6 mm. Hj}
8.63 Nsn#w
16.68 435450
84.86 8.14.2 Non* in
$SM tS &8&SB **
h-k 6S
>350 > 662
46 110
1.IM1 1.6517
4642 115-121
_
Mom is Sslfmy 3tfU
--
*9*46 14*151
1.664-1467
6*72 14*1*2
-
Dtt Whs point
Umtts
*66-165 208-222
1468-1485
150-170 Ml 302-338 (*!
-
328( 4586 mn
M64N (t60*5: 71Q
66.166
300-400
mm (266V; 138*8}
"
t f
0476038 f
TOWOLDMON0033008
ftMkr
M tt* Afodor piasttmw* *s {wavier than water, a valuable property for many apptieatfon*. Densities are shown in f%a 1.
#
e <6 K lit M HI M W M t M
Twnpsmtuw, *C Fig. 1 - Otadties el AreeM* ?tafeers m Varies* Tempsrstsfe*
I
Spedfie Vsltas#
Tie speeufc volume of Awsdor 124$ at different temperatures is m follow*:
TtmpsMm tfj
Atetlm tM Vakm (miff
0 0.674
.m e.m m s.m m sm m 0,828 m lift
0476039
TOWOLDMON0033009
The low vaptraatfan bm oi Aroclor ptatiozere is indicated to TaW* 8.
TASlt a
mmaxtm mm m mmm cusiiozEfiS
feeder 1221
tiJtsf, em.)
88.1m m
MfH
lapmm *tmc
24
kmSrntm
0.1872
24
Andwtttt MkarwnftctTowrt 1154'1fv8
turn
24 24
Ctmiw`M-%
mm
41
I
1
, 8JBS8 `
48
B&m** U
G.925S
24
mtfrnW*
U1M
24
matem/iM
, 0.0047
24
AmfwttU
0.IKJ35
24
1 1
- 0.0026
24
Arsdw 44*5 Are^or S442
8J3M , o.ooss
72 72
Aresstii 546C
mn
72
7V;*M iihatphaie
9.tKti
24
8m
mm mm* 0.000338 until 0.000128 8JBM1? 8.000087 9,000053 0,000810 0.000013 0,000008 0.000007 0.000084 0.$HH4 0.000003
It concluded that the vaporisation rate* of Arodor plasticizers -- espechuiy the most widely used 1254 and 1260 -- compare most favorably with the similar constants of other plasticisers selected specifically for these tots because of their low vaporisation rates.
0476040
TOWOLDMONOQ33010
The vapor pressures ef rreri Aroeior plattknw* are indicated in figure t over ft# tanprature range 150 to SWC. .
^i*T,K
Hg.1 -- Vapor Ft*wi sf Aroeior* Mssttows
The MimAei vapor pressures of serend Aroclor piastieizara at 10G"F shown in the following taisie were determined by extrapolation from the value* shown in Figure 2.
Apptexmats tper Pmstm efAtmfe/ Phstkkan htimtMti WPffflr CJ
Arerfar 1232
4.982 me. Hg
$m mm.
ktck-im
3.00037 am, Hj
Are*r 1254
3.88808 a*. g
0476041
TOWOLDMONOQ33011
The vtaas*tis of the Arodor ptotisiaers vary according to whether the hss* material a Mpbenyl or * poirphenyl and on the decree of chtwtiwtMh la general the lowndiiortnated biphenyls have the towwt vtaeoaMai {Figure $>.
fi*.3-Vitality 8aagn *t Sww Areeter# Wanted**
11 0476042
TOWOLDMONOQ33012
I
TlwWly M Mi
At ordinary temperatures A# Aroclor chlorinated polypheny!* haw not presented industrial toxicological problems. The hazard of potential toxic exposure varies with their volatility; the tawer-chtorinated, more.voUtik ones present more of a potential problem from the standpoint of both inhalation and skin contact When Arcelor plasticizer* are used at elevated temperatures, engineering controls must be applied, ether by the use of dosed systems or by elective local-exhaust ventilation iog^tfoer with ggfigyal workroom exhaust.
Vapor of the liquid Aroclor plasticizers at room temperature should not be breathed in a confined space, and no vapor of any Aroclor evolved at elevated temperatures should be allowed to be dispersed into the general workroom.
Inhalation tests on animals indicate that the maximum safe concen tration of vapor is in the range of from 0.5 to 1.0 milligram of the lower-chlorinated Aroclor plasticizer* per cubic mete of air. the threshold limit values (maximum allowable concentration for an 8* hour working day) set by the American Conference of Government Hygienist* are 1.0 milligram of the lower-chlorinated Aroclor cowpounds per coble mete of air and 0.5 milligram of tbe more-higblydrtorinated compound*, tmeb at Aroelor 126*, par cubic meter of air.
Schwartz patch teste on 200 volunteers showed that Aroclor 1254 waa neither a primary s'dn irritant or a sensitizer.
Prolonged or repeated skin contact with the Arcelor plasticizers must be avoided by tbe use of gloves and protective garments, because of the possible oceurrenbe of a condition called chloracne. Although re port* of this condition caused by Aroclor are rare, it can be produced by excessive skin contact. If any Aroclor is spilled on tbe skin the skin should be washed in the used manner with a soap solution,
A burn caused by contact wits a hot Arocior should be treated like any ordinary bam. Aroclor plasticizer adhering to tbe burned area need not be removed immediately, ante treatment of tbe bum demand* it, in which ease either soap and water or repeated washings with a vegetable otl are recommended.
i
n
0*760*3
TOWOLDMONOQ33013
Arcelor 1232, Aroelor 1242, Aroelor 1248, Aroelor 1254, Aroelor 1280, Aroelor 1282, Aroelor 1268, Aroelor 4465, and Montar 1 all contain polycMorinated biphenyl* <FCB) of various types and in varying amount*, PCB residues in small amounts have been found in the environment and some studies have indicated that they may be harmful to certain forms of animal life. Extreme care should therefore be taken by all user* of PCB-containing products to prevent any entry into the environment through spills, leakage, use, disposal, vaporisation or otherwise. Further, the products in which PCB materials are used, or which ar* formulated rising PCB materials a* a component, should be given careful study to eliminate the possibility that PCB might reach the environment as a result of use in a given application. Some specific applications where the use of PCB should definitely he avoided are in paints and sealants for swimming pools, paints and waterproofing agents p silos and other buildings where food products for humans or animals are steed, and as a component of any container or wrapping used in the packaging of food products.
0476044
13
TOWOLDMONOQ33014
4
Prm$A ChmipMim
Arodor 1221,1233,1242,
Synthetic Resin, Liquid, NOIBN
1248,1254,1260,1262
Bn# Ctemfimtim
Aredor 1268, 4465, 5442,5460
Synthetic Ruiu, Other Than Liquid, NOIBN
IMt Cta#ca0
Arcelor 1268 Arodor 4485, 5442,5460
Synthetic Resin, Powder, NOI
Synthetic Resin, Lumps or SoW Mass, NOI
Shipping BcgtdMiam
None
Standard Container* Arodor mi
Arodor 1282
Arodor 1242,1248,1254, 1280, 1268
Afodor 1268 '
Arodor 4468 Arodor 8442 Arodor '>460 (flaked)
Tank car, 5204b. steel dram, 604b. eon
Tank car, 6604b. sted drum, 604b. cm
Tank ear, 6004b. sted drum, 604b. can
200-lb. fiber drum, 25-lb. fiber dram
600-lb. sted drum, 50-lb. can
1134b. steei drum, 60-lb. can
504b. bag
0476045
TOWOLDMONOQ33015
DISTRICT SALES OFFICES All DIVISIONS ! **
AARON, OHIO 44313
m
am isio*
7ft. <218) 8*8-4111
_!
ATLANTA. GEORGIA 30326
Lmtm Timms tm
3400 Pmctt'f 68. ft. . - Sum-1711
M 1404) 077-2300
J m (Ziff 423-9031
J ot$ mw*s, towa sojio
< J
313 Mtte Way T
m w*i
BOSTON, MASSACHUSETTS 0214$ immmsuim W. 307-6010
CHICAGO, ILLINOIS
PiwnwAm. /%*** imrms 80018 r* /sra; 290*0888
CiNCmmTK OHIO 45206
7567 Ma&tsm ftmtf TH 1513) 151-6101
Demon, Michigan
SCO Nonhtmo Tewms wtt SuvtMhtd, Mtch. 46076 rt r3M 367-oato
HONOLULU, HAWAII 96812 206 PtdHt IMwmUeml 818). err A* Hm SM, P. 0, 8m 3874 18L 1000)631-2748
HOUSTON, TEXAS 77027
138! Pmt OM T&wsr SOS? Wamakmr Bmd 7ak iJi$) 021-8080
LOS ANOSUS CAl IFORNIA 90022 moe.fieumst. TH, 1213) 723-2432
mw tom, nsw took 10017
277 Park Avaum 7*1 {212} 822-4111
>/, U':ntS, Afm >j*u mw
800 N. UnmfV* 8m tat. t'3U1 m* JQQO
SAN ffiANCtSCO SAY ABEA
27tQLtfy*t, Santa Oars. Cam. 88052 TH {408} 242*0414
SAfTL, WASHINGTON 98121 2112V**Awmut 14.1X0) 622-4203
WILMINGTON. DELAWARE 19603
tom Cancwt) Pike, etifitx m. '302) 658-5531
J ;
m yma ni-nm Indianapolis Indiana msm
SuR* 215. 4062 Mttrftw* 0* {MSfev T#l {31?} 647-Si48
j
KA7N01SA6Sh#CIRTwYS,gaMtoISwSOfURI 84133 4240 Bte* R9g# SealaviSfd
m (m asa-soeo
J LOUNG. LOUISIANA 70070
*
P. 0- Bfi* 174 m (6041 784-S2S3
j
MANKATO, MINNESOTA 59961 mmsm&fiMM
* m (607J 387-3408
i
. TENNESSEE 39104 SwiWtna
J T*L (901)278-7911
\ * J
MUSCATINE. IOWA 62781 P,O.Be*473 m (3181 283-1331
*
I
J J
*
t. 01081 Ti(413) 3 (Am Q4 it DORADO. ARKANSAS 71730 UmMmtMnv
% Ti. (601J 683-3111
'J
JAPC.KOS.O9Ne,* M16I8S3S7IS, SIPPI 3S20S 7*1.(90113524648
$ H. LITTLE ROCK. ARKANSAS 73118 410War, m sat P. 0. Sax 6821
t i
f#L (#011 378*2437 MIMPHI8. TENNESSEE 3811*
1023 Kmmte* Ottos, 9. 0- Box 13248
* T*L (9011 948-4461
t i ft#**#* siritiwi \ . OREGON 97402
%
TL (803) 343-7201 KENNoILtWh O$RT*H*.*N$EtW& JMEoRoSE>Y* A0m76*3
% Tat (2C1) 278-2900
i *
SPRiNGPicto. mass. 01 i<n P.6.9a 2136.
m (413) 788-4911
Txtii* Dh>i*l88
*
* J
ATAL6ANft{T*A GEORGIA M3a0o30
246 Acschtra* |t W
m (404) S77-22W ' CHARLOTTE NORTH CAROLINA 28240
l 62*0 7**v>< Road. 400
S *
m <7041 366-0116
6RESNVIUL. SOUTH CAROLINA 28908 P|NI
P. O. 9e* 6884, Smkm S
* i
Ti f2i 239-9171 NEW Y0H NEW YORK 10001
3S0 fm Am T*L (212)
MONSANTO. S60 N. UNOBmH BLVO., sr. iouis. M/ssomi mss