PLASTICS COMMITTEE MEETING The Greenbrier
White Sulphur Springs, W. Va. June 8, 1961
PRESENT: Messrs,
Walter H. Salzenberg, E, I. du Pont de Nemours & Co. Earle S, Ebers, U. S. Rubber Company W, C. Goggin, The Dow Chemical Company W. C, Lowrey (for Martin Buck) Shell Chemical Co. W. P, Marsh, Jr., U. S. Industrial Chemicals Co. T. T. Miller, W. R. Grace & Co. R, J, Nelson, Enjay Chemical Company F. M. Norton (for T. J. Kinsella) Allied Chemical Corp. J. C. Searer, Hooker Chemical Corp. R, K. Turner, Union Carbide Plastics Co. Harry B. Warner, B. -F. Goodrich Chemical Co. David C. Williams, Eastman Chemical Products, Inc. H. R. Dinges, Spencer Chemical Company E. J. Sullivan (for A. R. Marusi) The Borden Chemical Co. H. W. Mason, Jr., Reichhold Chemicals, Inc. R. K. Mueller, Monsanto Chemical Company Henry Avery, Pittsburgh Chemical Company W, C. Brown, Hercules Powder Company George Wash, Phillips Chemical Company P. H, Carman, MCA William Demarest, MCA
The meeting was called to order at 8:20 A.M., with W. H. Salzenberg in the chair. The Secretary announced that 40 members of the Plastics Group (10 had not returned a ballot) cast unanimous votes for four new Committee members: H. R. Dinges, A. R. Marusi, H. W. Mason, Jr. and R, K. Mueller; appointment of these new Com mittee members, together with W. H. Salzenberg as Chairman and I, T. Miller as Vice Chairman, was confirmed by the Board in its meeting the previous evening.
Following welcome to these new members, to E. J. Sullivan ^presenting A. R. Marusi, to W. C, Lowrey representing Martin Buck and to P. M. Norton representing T. J. Kinsella; and, to jkcry Avery, W. C. Brown and George Wash, present by invitation, tbe Secretary commented briefly on Terms of Reference (approved by the Board in 1952) pertaining to the Plastics Committee's activities. * digest of these Terms is attached as Appendix A.
fLASTICS FINANCIAL PACKAGE
. The estimate of 1960-I96I expenditures was forwarded to memr Executive Representatives on May 15* together with ballot' for * Committee members and individual company assessments for the
CMA 078445
2
new fiscal year. Total expenditures for 1960-1961 were $70,105,17 (estimate of May 15 was $70,033) and the actual deficit was $828.25 (originally estimated at $756),
The budget for the next fiscal year, previously approved by the Committee, totaled $72,500. Assessments to collect these funds were included in aforementioned letter to Executive Representatives;
it was concluded this budget and assessments were acceptable and statements will be forwarded to members except where payment has
already been received.
PLASTICS -- INSTITUTIONAL SEATING
With W. C. Brown and George Wash being present, all companies interested In this problem and participating in the May 4 meeting were represented at this Committee meeting. Mr. Wash commented briefly on the results of flammable tests conducted by Phillips Chemical Company and as reported to the SPI Board in their recent meeting. A copy of their laboratory's report is enclosed, together
with comments by P, X. Ambrose, Chairman of the SPI Code Advisory Committee (Appendix B).
It was the consensus of those following this problem that the plastics industry should limit activity to that of the Code Advis ory Committee and technical aspects at this time. The opposition to use of plastics appears to have been materially ameliorated and further contacts on an industry-wide basis can be handled better by the Code representatives and the Consultant on the West Coast.
UNDERWRITERS' LABORATORIES PROJECT
There have been no major developments since the May 4 Committee meeting. Samples of a self-extinguishing vinyl chloride sheet material have been supplied the V/L for further evaluation as a drip pan and grille In air conditioners -under test.
The proposal of Baron Whitalter, Vice President of Underwriters' Laboratories, that the plastics industry committee continue liaison with the Laboratories and assist them in evaluating plastics for
building, and the action of the Plastics Committee in February on a related subject were reviewed. On May 4 it was the consensus that the work should not be terminated abruptly on completion of the project now in the U/L and that It would be In the best interests * the industry for the committee technicians to continue a working
or consultative relationship. With a view to maintaining this liaison with the Laboratories, the Committee endorsed the suggestion that the MCA staff, together with the chairmen of the U/t* Advisory Committee and possibly of the Plastics in Building Committee, con
sult with Mr. Whitaker at an appropriate time.
RUSTICS IN BUILDING
CMA 078446
Mr, Demarest reported that the new Steering Committee (W. P, *arsh, Jr,, T. T, Miller and R. K. Turner) had been supplied details
hi'* v Plastics in building program to date; this Steering Committee a been invited to meet with the Building Committee on June 14.
Messrs, T. T. Miller and W. Demarest reported that the MCA and SPI contributions to the Annual BOCA meeting had been graciously acknowledged by Philadelphia Building Inspector Lieberman In an ad dress in the SPI Annual Meeting earlier this week.
In reporting on the plastics aspects of the Building Research Institute Spring Conferences, William Demarest commented on the value of Intersociety reports by the various Industry organizations active In plastics in building.
Members' attention was called to a recently published volume on "Industrial Building" covering proceedings of the December i960 Industrial Building Congress (232 pages) which Includes a discussion of new developments in application of plastics to industrial con struction by William Demarest.
OYSTER HARBORS CONFERENCE
Henry Avery, Chairman of the Arrangements Committee, commented briefly on the plans of the group to follow through on suggestions already supplied by the Committee in the May 4 meeting.
The suggestion made sometime ago that speakers be used on one morning only In an effort to obtain better attendance was then con sidered. Following a full discussion, it was voted that the Com mittee should obtain speakers for a one-morning session and that the Washington office advise Executive Representatives that this arrangement was made with the view of having a better attendance for the speakers and that the Executives be asked to do everything possible to have registrants attend.
ANNUAL MEETING -- PLASTICS GROUP
In view of the limited capacity of the Greenbrier's President Buchanan and Fillmore Rooms for the Annual Dinner meeting, the Secretary was authorized to propose that the evening dinner meeting be moved to the Gates Mountain Lodge, with the understanding that the business session will be terminated in time for registrants to join the Association activities scheduled later In the evening.
**#*#*-#****
Member representatives attending the dinner meeting are -isted in Appendix C. The program included (l) welcome by Chairman V h. Salzenberg, who expressed regrets of T. J. Kinsella in not "e*nE able to be present, (2) remarks by MCA President J. E. Hull, (^statement of appreciation for services of members who had com?*eted their terms on the Plastics Committee -- namely, Earle S.
"2ers, J, c. Searer, Harry B. Warner and David C. Williams,
CMA 078447
4-
(4) introduction of new Committee members, {5) announcement of mem bers appointed as a steering group to maintain liaison with the SPI on building programs, and (6) announcement of the Arrangements Com mittee for the Oyster Harbors Conference, September 7 and 8, 1961,
Members were advised that the Plastics Committee ordinarily meets the second Tuesday of each month during the winter; the next meeting is scheduled for September 8 at Oyster Harbors, Executive Representatives were again reminded that they are always welcome to attend these meetings for a discussion of industry problems that warrant consideration by the Association. MCA Bulletins regularly carry announcements of forthcoming meetings and matters of general interest to the Plastics Group,
ADJOURNMENT
The dinner meeting adjourned at 9*15 F. M.
FHCiew
Enclosures
Committee Secretary
cc; Mr. A. Lloyd Symington Executive Representatives of Plastics Group and Alternates
June 15, 1961
CMA 078448
Manufacturing Chemists' Association, Inc. June 20, 1952
TERMS OF REFERENCE PLASTICS
Appendix A
The Board of Directors approved a resolution setting up certain Terms of Reference governing formation and. activities of the Plas tics Committee. These were approved in the early part of 1952 by the Plastics Committee. Pertinent provisions of interest are:
1. Members shall be appointed on a rotating basis with the objective that they do not at any time represent in num bers or volume of production a predominant position in
the industry or any major segment,
2. The Committee is authorized to select its own chairman,
3. The Committee may make oral reports of its activities to the members twice a year at regularly scheduled sessions in conjunction with the Association meetings. Any other reports other than those at such special meetings as may be authorized by the Board shall be
in writing.
4. The Committee is authorized to represent the manu facturers on broad problems arising from activities of Government agencies, etc.
5. The Committee is authorized to sponsor and make avail able technical literature as may be required.
6. The Committee is authorized to promote safety in the manufacture of plastics utilizing to a maximum ex tent the existing committees of the Association,
7. The Committee is authorized to participate in volun tary standardization programs with respect to color and the like in cooperation with the Commodity Standards Division of the Department of Commerce, and to maintain liaison with A.S.T.M. on similar
programs.
8. The Committee is authorized to continue to encourage and participate on a voluntary basis in a fundamental research program such as that at M.I.T.
9* The Committee is authorized to collect statistical data pertaining to volume of production and past transactions or activities as required for specific,
non-routine purposes,
^ all instances these activities of the Committee and the Plastics 'jj'oup muS be consistent with the By-Laws, The above-mentioned ac
tivities were carried on by the former association and it is under stood that they would be so conducted in M.C.A. on the same basis was the practice in P.M.M.A. The only important departure from
is frequency of general meetings.
CMA 078449
Appendix B PHILLIPS CHEMICAL LABORATORY Tests on Materials -- Plastics Seating
C
0
P
Ignition Temperature
There are a number of methods (1,2,3) contained In the litera ture for determining the ignition temperature of solid materials. Due to obvious time limitations, however, the technique we employed to evaluate the Ignition temperatures of our materials was In use in research. In operation, approximately 0.06 gram of the mater ial In question is placed in a small steel crucible which is con tained In a Ramsbottom furnace. The temperature of the furnace Is then increased gradually-and the temperature at which the material
"flashes'* was arbitrarily designated as the autoignition tempera ture, Using this procedure, we determined the ignition temperature on MARLEX*, impregnated plywood, conventional plywood, polypro pylene, fiberglas filled epoxy, Kralastic and wood impregnated melamine. The results of this study are shown below:
Material
Autoignition Temperature, F
MARLEX Impregnated Plywood Plywood
Polypropylene Fiberglas Filled Epoxy Wood Impregnated Melamine Kralastic
900 900
950 950 950
1025 1025
It should be realized that due to the Inability to measure this ignition under precise conditions these data should be con sidered as only approximate. For more precise results, it is sug gested that ignition temperature be determined according to the method of Setchkin (l). Nevertheless, this data can be used as a yardstick to compare the relative ignition temperatures of plastics. Incidentally, the many building codes classify a material as com bustible if it will Ignite when exposed to a temperature of 1200 or 1380 for five minutes. Needless to say under such a classifi cation very few plastics would be considered as non-combustible.
Burning Tests:
The most widely used burning test for measuring the flamma
bility of plastics is the ASTM D635-56T method. In this method, a
specimen of known geometry Is Ignited and the rate of flame front
travel between two previously marked gage lines on the test' speci
men is subsequently determined. The results are usually reported
In inches/minute. A plastic material is designated as "slow burn
ing" if the burning rate Is less than 2.5 inches/ninute, This
procedure was used with the same materials as described previously
^<3 the results are tabulated below:
'
A trade-mark,
(Over) CMA 078450
Material
Burning Rate -In-, /min.
- Comments
Kralastic
1.2 Very much soot and smoke, drips
Natural MARLEX
1.0 Melts, drips, candlewax odor
Polypropylene
0.8 Burning area transparent, swells, drips, heavy
sweet odor
Flame Retardant Coated MARLEX
0.7
Melts, drips, waxy odor
Fiberglas Filled Epoxy
0.7 Much soot, phenolic odor, does not drip
Plywood
Self extinguishing
Impregnated Plywood
Self extinguishing
Wood filled Melamine
Non-burning Merely glows
Another widely used burning test for classifying materials is ;
Underwriters' Laboratories tunnel test. This method which is de- 1
scribed in various standard test procedures (4,5,6) consists of
*
burning a section of material, twenty-five feet in.length and twenty_
inches in width, under controlled conditions and subsequently measur
ing the flame spread. Comparing the burning rateof the material to j
red oak which has aflame spread index of 100 and cement asbestos 1
which has a flame spread index of 0, a rating is then assigned to I
the plastic material. Due to the high equipment costs which would 1
be necessary to conduct this test, MARLEX was not evaluated." How
ever, since some model codes now include plastic materials on the
basis of a flame spread index, it would be advisable to obtain such
data. Underwriters' Laboratories in Chicago has the necessary equip
ment to perform this evaluation. Incidentally, the Uniform Building
Code also approves plastic materials which have a flame spread
rating of 225 or less according to UBC Standard #52-l-6l. Since we .
did not have access to this particular procedure, it is not known j
whether this rating applies to the UL test or is a distinct flame
i
spread rating procedure.
;
Another fire test which 13 used quite frequently is the "Standard
Methods of Fire Tests of Building Construction and Materials."
j
These tests, which are primarily applicable to assemblies of masonry I
units and to composite assemblies of structural material for build- *
ings, prescribe a standard exposing fire of controlled extent and
severity under which fire resistance is determined in tenns of
i
hours or fractions thereof.
*
CMA 078451
The temperatures involved in this test range from 1000 P to greater than 2300 F, For this reason, very few thermoplastic
materials could be expected to pass this test.
In order to simulate some type of fire endurance test and at the same time obtain some indication of the effect that wax drip pings from MARLEX would have on flooring material, three MARLEX seats were mounted 18" above three different types of flooring materials which included oak hardwood, vinyl tile and rubber tile. The seats were ignited at the outer edge by means of a bunsen burner, and photographs were then taken during a period of fifteen minutes. Figures I through III provide a graphic illustration of
this test. You will note that even though the drippings did set the vinyl and rubber tile on fire, it was restricted to a specific area. Figure IV illustrates the effect of flame retardant coating. Both sides of a MARLEX seat (right side of which was treated with flame retardant coating) were ignited by means of a bunsen burner for the same period of time. You will note from Flgire IV that after approximately one minute the flame was extinguished on the side with the coating while the uncoated side continued to burn.
Miscellaneous Tests:
(a) Drip Test
Underwriters' described what is referred to as a "drip test"
in which they measure the time it requires for a melting droplet
of flowing material to fall after a one-minute application with a
bunsen burner. According to Underwriters' Laboratories who per
formed this test on MARLEX conduit, our material would be consid
ered unacceptable at such time that the National Electrical Code
would be revised to permit limited use of exposed nonmetalllc
conduit,
'
, '
(b) Products of Combustion
No standard test method has been developed for measuring the combustion products of burning materials because of the lack of information on the mechanism of uncontrolled combustion. However, for MARLEX polymers, the principal combustion products that would be formed would be water, carbon monoxide, carbon dioxide and oxygen. The relative percentages of each that will be formed will be dependent on the degree of combustion. Some codes specify that
oaterials would not develop gases more toxic than wood or paper where burned under similar circumstances. Under this general classification, MARLEX would probably be acceptable.
, v CMA 078452 (c) Smoke Density
Uniform Building Code has a restriction on the smoke that can
r* tolerated for an approved plastic material. A plastic material r approved must have a smoke density not greater than that obtalned from the burning of untreated wood under similar conditions when tested in accordance with UBC Standard #42-1-62, Although we nb have a copy of this code, it is recommended that we purchase ^ standard test volume so that we can rate MARLEX.
(Over)
Another method available for obtaining some indication of
smoke intensity is by the use of the tunnel test in which the smoke generated during the test is quantitatively determined. However, there is some question whether this method is satisfactory.
Recommended Future Tests
-
(1) Since some of the Building Codes now require a maximum flame spread rating for plastic materials, it is suggested that we enlist the services of Underwriters' Laboratories in Chicago to run a tunnel type evaluation on MARLEX, .
(2) Since fire officials place a great importance on smoke
released, we should obtain a copy of Uniform Building Code Standard
#42-1-61 and obtain a comparison of smoke density of MARLEX vs,
;
wood.
i
(3) Although toxicity of products of combustion should not be .
a problem, we should enlist the aid of Research to obtain quantita- J
tive results on combustion products of MARLEX. In addition, we
\
should check with either SPE, SPI, or Manufacturing Chemists' Asso- j
elation to ascertain which test method to employ.,
j
(4) Since the ignition temperatures as determined by Research ) are only relative, we should repeat the test using the method of Setchkin. Perhaps we can have Underwriters' obtain these results ' since elaborate equipment is needed here also.
*#**#**#***
" BIBLIOGRAPHY
1
(1) Journal of Research of the National Bureau of Standards, . Vol. 57, #4, October 1958.
(2) Modern Plastics, Vol, 20, #6, February 1943.
(3) A5TM Bulletin #151, March 1948.
..
'
(4) NFPA Bulletin #255.
(5) UL Bulletin #723.
(6) ASTM #E84,
i
! 1 I
This report prepared by Mr. Jones and supplied through courtesy of Mr. George Wash.
Copied by Manufacturing Chemists' Association, Inc. June 15, 1961
CMA 078453 *
FIGURE I MARLEX SEAT IGNITED ABOVE A HARDWOOD FLOOR
V f" r
-- r nl ----i-^* CMA 078454
T "
FIGURE 3
marlex seat ignited above a rubber tile floor
CMA 078456
SmI
" T "'
.Appendix B Comments by F. X. Ambrose, Chairman, SPI Code Advisory Committee*
There are a few details which I might clear lip for Mr. Jones. On Page 3, reference is made to UBC Standard 52-1-61. This is merely a reference to the Manufacturing Chemists1 Association's book en titled "Technical Data on Plastics", current edition. The section of the Code in which this reference is contained, deals with identi fication and approval of plastics, and reads in part as follows: "Approved plastic materials shall be those specified in U.B.C. Standard No, 52-1-61 which have a flame-spread rating of 225 or less" ...etc.
The Tunnel Test is the Underwriters1 standard procedure. On Page 4, reference is made to UBC Standard No, 42-1-61. This is identical with the Underwriters' Laboratories"Tunnel Test.
In general, I think that the data which has been developed is favor able, Undoubtedly, the photographs would be disturbing to regula tory authorities, yet it is a universally accepted fact that there is no tendency for flame to travel across the surface of a floor. Hence, burning material on a floor can be considered relatively harmless.
In addition to the testing work which has been done or which has been recommended for future action, I would suggest that some data on heat of combustion be developed. The BTU's per pound of the Marlex could then be compared to the BTU's per pound of wood furniture, and the total design could be taken into consideration. It should be pos sible to develop a figure for BTU's per chair, molded plastic versus plywood or wood. The potential BTU release from a classroom fire, should be a very important factor, I say this, because I don't see how flame-spread could be a factor since there is no continuous sur face over which flame could travel.
As a matter of fact, it would be my personal recommendation that the question of furniture standards or approval be kept as far as possible removed from any connection with building codes. Certainly, building codes are not intended to deal with furniture, and drawing the Build ing Departments into the picture might only serve to complicate the problems.
On the last page of Mr. Jones' report, there is mention of tests for toxicity (Item 3), This is a subject on which a fair amount of study has been conducted both by industry groups and, more recently, by the Code Advisory Committee. The fact of the matter is that extremely little is known about the exact cause of death where fire and smoke are involved. While casual newspaper and fire reports may attribute death to asphyxiation, smoke poisoning, carbon-dioxide (or monoxide), txygen starvation, or hot gases, etc., all such statements appear to he opinion or conjecture. This undoubtedly accounts for the lack of any standard test for toxicity of combustion products. Where author ities have insisted on toxicity information, we have generally been able to resolve their questions with tests on white rats. A sample wst report is enclosed. This type of test, plus an analysis of com bustion cases, would certainly Indicate whether or not noxious gases 4re given off in any harmful quantities.
CMA 078458