Document ykKe4mq0po7NQxx35Exma2OK6
TECHNICAL
BULLETIN
if
SW 379643
STLC0PCB4100415
AROCLOR PLASTICIZERS
A series of inert, chemically-resistant, fire-retarding plasticizers compatible with wide variety of resins. TECHNICAL BULLETIN O/PL-306
PLASTICIZERS
"Nothing contained herein Is to be construed as a recommendation to use any product in conflict with any patent. MONSANTO MAKES NO WARRANTIES AS TO THE FITNESS OR MERCHANTABILITY OF ANY PRODUCTS REFERRED TO, no guarantee of satisfactory results from reliance upon con tained information or recommendations, and disclaims all liability for any resulting loss or damage."
Organic Chemicals Division / 800 N. Lindbergh Blvd. / St Louis, Missouri 63166 ;
DSW 379644
STLCOPCB4100416
Table of Contents
INTRODUCTION................................................................................. 4
DESCRIPTION...................................................................................... 4
COMPATIBILITY................................................................................ 5
AROCLOR IN SYNTHETIC RESINS........................................ 6 Polyvinyl Chloride...................................................................... 6 Polyvinyl Acetate......................................................................... 13 Ethylene/Vinyl Acetate...............................................................14 Epoxies........................................................................................... 15 Polyesters.......................................................................................18 Polyethylene................................................................................. 19 Polystyrene................................................................................... 19 Polyurethanes............................................................................... 20 Phenolics........................................................................................21
AROCLOR IN RUBBERS...................................................................21 Chlorinated Rubber and Polypropylene....................................21 Styrene-Butadiene Copolymers.................................................. 23 Synthetic and Natural Rubbers................................................. 24 Polysulfide Sealants..................................................................... 26
AROCLOR IN CELLULOSIC RESINS............................................27 Ethyl Cellulose............................................................................. 27 Nitrocellulose................................................................................ 28 Cellulose Acetate-Butyrate......................................................... 31
AROCLOR IN PAINT, VARNISH, WAX, AND ASPHALT. . .32 Paint and Varnish........................................................................ 32 Wax................................................................................................ 34 Asphalt...........................................................................................35 Ally] Starch................................................................................... 35
AROCLOR IN MISCELLANEOUS APPLICATIONS.................. 36
Dust Prevention and Dust Catching......................................... 36
Vapor Suppression (Longer-lasting Insecticides)......................36
Moisture Proofing.........................................................................36
Pigment Dispersion..............
37
Sealing and Impregnation............................................................37
DSW 379645
STLCOPCB4100417
t'
PROPERTIES OF THE AROCLOR PLASTICIZERS.................39 Solubility.......................................................................................39 Chemical & Physical Properties (Chart)............................42, 43 Monsanto Specifications.................... .................................42, 43 Density.................................................................................. ... 44 Specific Volume............................................................................ 44 Volatility....................................................................................... 45 Vapor Pressure................................................................... Viscosity........................................................................................ 47 Stability.........................................................................................47 Nonflammability...........................................................................48 Nondrying and Thermoplastic Properties................................. 48 Electrical Properties.....................................................................48 How to Emulsify Aroclor............................................................ 49
46
TOXICITY & SAFE HANDLING............................................... .50
SHIPPING...............................................................................................51
DSW 379646
STLCOPCB4100418
Introduction Description 4
The unique Aroclor plasticizers are among the most versatile chemi cally produced materials available. One outstanding characteristic -- inertness -- makes Aroclor useful in many ways for many different applications. The major benefits offered by Aroclor include:
Chemical Resistance Fire Retardance Compatibility with most resins Nonoxidation Adhesivity Low Cost
This bulletin describes some of their many important plasticizing and related applications, including numerous suggested starting formula tions. Examination of their physical properties, also given in consider able detail, may suggest scores of new uses that could not be performed by any other known material.
Additional information about the Aroclor compounds is available from your nearest Monsanto district sales office in the following technical bulletins: PL-307.............. Monsanto's Plasticizers in Synthetic-Resin Adhesives PL-311.............. Aroclor Plasticizers for Chlorinated Rubber PL-321.............. Aroclor 1221,1232, 1242 for Polyvinyl Acetate Emul
sion Adhesives PL-327.............. Monsanto's Plasticizers in Protective Coatings PL-331.............. Monsanto Modifiers for Polysulfides CS-14................ Aroclor Fire-Retarding Plasticizers and Modifiers in
Epoxy Resins CS-18................ Aroclor Compounds (performance with waxes)
Monsanto's Aroclor plasticizers comprise a series of chlorinated bi phenyls and chlorinated polyphenyls. They vary from mobile, oily liquids to white crystals and hard, transparent resins.
Twelve of the Aroclor plasticizers, each of which represents a series, are discussed in this bulletin. An understanding of the system for designation of each Aroclor should prove useful in the evaluation of the property gradations among them. The last two digits indicate the approximate weight percentage of chlorine in the product, and the first two digits indicate the type of material, as follows:
12 -- chlorinated biphenyls 25 -- blend of chlorinated biphenyls and chlorinated triphenyls
(75:25) 44 -- blend of chlorinated biphenyls and chlorinated triphenyls
(60:40) 54 -- chlorinated triphenyl3
For nearly every Aroclor mentioned, a darker, less-pure grade exists, with about the same physical and chemical characteristics, but lower in price.
DSW 379647
STLCOPCB4100419
Compatibility
Aroclor compounds are nonoxidizing, inert, permanently thermoplastic, of low volatility, non-corrosive to metals, and low cost. Aroclor com pounds are not hydrolyzed by water and resist alkalies, acids, and corrosive chemicals. The viscous, more-highly-chlorinated liquids and resins do not support combustion, and they impart fire retardance to other materials.
The crystalline Aroclor compounds are relatively insoluble, but the liquid and resinous compounds are soluble in most of the common organic solvents, thinners, and oils. All Aroclor compounds are in soluble in water and glycerine. Aroclor 5460 is insoluble in lowermolecular-weight alcohols; Aroclor 4465 is only partly soluble in the lower alcohols.
Aroclor compounds plasticize a great many resins without softening them unduly. The Aroclor compounds are unsurpassed for the plasti cizing of protective coatings, particularly for use in chemical plants and other facilities that require a tough, chemically resistant surface. Aroclor plasticizers can also be used to flexibilize sealing compounds, adhesives, lacquers, inks, varnishes, free films, fabric coatings, and pigment dispersions. They are also used as components or extenders in elastomers and waxes. The properties of many end products can be improved -- yet at reduced overall cost -- by the use of an Aroclor as either a primary or a secondary plasticizer.
The properties imparted by Aroclor compounds (and their usefulness in particular applications) vary in regular gradient over the series. Selection of the right Aroclor for a particular use can generally be made by comparison of the properties, by "blending" two or more, and by adjusting the percentages used in the particular mixture in which the Aroclor compounds are formulated.
Monsanto's Plasticizer Council can provide specific formulation guidance that may help you improve your product or lower your processing cost. Processors are invited to ask the nearest Monsanto office for help on special problems.
The Aroclor plasticizers are compatible with most common plastic materials; they are compatible to the extent of practical use with the following:
Asphalt Benzyl Cellulose Camauba Wax Cellulose Acetate-Butyrate Chlorinated Rubber Coumarone-Indene Resins Damar Resin Ester Gum Ethyl Cellulose Ethylene/Vinyl Acetate Epoxy Resins Nitrocellulose Paraffin Phenolic Resins
Polyethylene Polyester Resins Polystyrene Resins Polyisobutylene Polysulfides Polyurethanes Polyvinyl Acetate Polyvinyl Butyral Polyvinyl Chloride
Polyvinylidene Chloride Rosin Rubber Styrene-Butadiene Copolymers
DSW 379648
5
STLCOPCB4100420
Liquid Aroclor
Soft, Resinous Aroclor
Hard, Resinous Aroclor
Aroclor plasticizers are not compatible with phenolic resins in the final stage of condensation or with cellulose acetate. Aroclor plasticizers generally impart progressively increasing proper ties in the direction of the arrows in the following diagram:
Flame Hardness Flexibility Retardance Volatility Density Viscosity
Usually the desired balance between flexibility and hardness can be obtained either by selection of an Aroclor with the appropriate physical characteristics or by use of a blend of two or more Aroclor plasticizers. In evaluation of formulations that contain Aroclor plasticizers, the compounder should thoroughly test an experimental product for compatibility, heat and light stability, and other properties according to normal industry practices.
Aroclor Plasticizers In Synthetic Resins
Low-cost Aroclor plasticizers are valuable for a variety of applications. They improve chemical resistance, flame retardance, and oxidation resistance. Depending upon the use, the various Aroclor plasticizer offers a number of benefits to the user. In almost all formulations, the use of an Aroclor reduces the over-all cost per pound.
In Polyvinyl Chloride
Aroclor is valuable in polyvinyl chloride and copolymers as a secondary plasticizer or as a plasticizer extender. The Aroclor plasticizers impart flame retardance and chemical resistance.
Selection of the proper Aroclor enables compounders to impart such special properties to their formulations as:
Resistance to migration to nitrocellulose lacquers (Aroclor 1260 and 1262).
Fine, uniform cell structure in vinyl foam (Aroclor 1262 and 1268).
Adhesion in vinyl coatings (Aroclor 1260 and 5460).
Viscosity stability in plastisols (Aroclor 1248 and 1254).
Compatibility
Aroclor plasticizers (except Aroclor 1268) are compatible to about 25 per cent of the total plasticizer content in polyvinyl chloride and usually somewhat greater in copolymer resins. At these levels, no exudation occurs in the loop-compatibility test, one of the most severe used by the industry. .
DSW 379649
STLCOPCB4100421
The control specimen bums rapidly; the one containing Aroclor does not even ignite.
Performance
As an illustration of the performance of Aroclor plasticizers, Table 1 shows evaluation of the five most commonly used in polyvinyl chloride.
TABLE 1
PERFORMANCE EVALUATION OF FIVE AROCLOR PLASTICIZERS IN POLYVINYL CHLORIDE
Voia- *
Low-Temp
Hard- tiiity Kerosene-e Flexibility
Concern ness (Plasti- Extraction (Clash Tensile
Elonga-
tration (Shore cizer (Plasticizer & Berg) Strength Modulus tion
Aroclor (parts) -A") lost, %) lost, %) (Tf.. C) (psi) (psi) (%)
1248 15 87 19 23 -26 2330 1320 342
1254 15 88 14 24 -24 2310 1360 334
1260 15
89 11
32
-22
2200
1330
! Q9*3 K
-.1
4465 17.5 89
6
19
-19 -- -- --
5442 17.5 87
6
16
-20 - - --
Ingredients
a) Opalon 660 PVC resin Dioctyl Phthalate Calcium Carbonate Stabilizer Aroclor
b) 24 hours at 87"C over activated carbon
c) 96 hours at 25*C
Parts by Weight
100 45 40 3 indicated
DSW 3796SQ
7
STLCOPCB4100422
Heat and Light Stability
Aroclor compounds impart good heat stability but somewhat reduce the light stability of vinyl formulations, but no more so than do many other secondary plasticizers commonly used in the industry. Light stability of the system may be improved by incorporation of a small amount of light-screening agent, such as 0.1 per cent Tinuvin P.*
Chemical Resistance
For imparting resistivity to chemical attack, the Aroclor plasticizers are unsurpassed. Independent evaluations of the chemical resistance of vinyl chloride-vinyl acetate copolymer paint, modified by eight types of materials (alkyd resin, phenolic-chinawood oil varnish, ester gum-linseed oil varnish, Aroclor 1254, dioctyl phthalate, tricresyl phosphate, polymeric plasticizer, and acrylic polymer), showed that Aroclor 1254 has the "best all-around chemical resistance, failing badly only in the gasoline test."
Paints were sprayed onto solvent-cleaned, unprimed, cold-rolled-steel panels, which were then immersed in seven types of solutions until failure. The data in Table 2, excerpted from the November 1955 issue of Official Digest of the Federation of Paint and Varnish Production Clubs, compare the chemical resistance imparted by Aroclor 1254 and by dioctyl phthalate.
TABLE 2
COMPARATIVE CHEMICAL RESISTANCE OF PLASTICIZERS IN VINYL CHLORIDE - VINYL ACETATE COPOLYMER PAINT
Plasticizers
Dioctyl Phtha late (%)
10
--
25
--
40 --
Aroclor 1254 (%)
--
10
--
25
--
50
a) End of test
10% Sodium Hydrox
ide (days)
120*
120*
60
120*
60
120*
Time to Failure in Corrosive Media
10% Hydro chloric Acid Gasoline (hours) (days)
92 0.4
168* 5
24 0.4
120 0.4
24 0.4
96 0.4
5% Sodium Hypo chlorite (days)
4
13
4
14.5
4
11
Linseed 10% Oil Acetic Fatty Acid Acids (hours) (days)
84 60
168* 90*
84 27
120 90*
48 22
100 60
1% Tide at 160'F (days)
21 22
25
22
25
22
In other corrosion-resistance tests of polyvinyl chloride plastisols, containing 70 parts plasticizer per 100 parts resin a formulation that contained 1 part Aroclor 1254 to 3 parts dioctyl phthalate was much more resistant to 15 percent nitric acid at either 23 or 50C for six months than a compound plasticized with dioctyl phthalate alone.
The plastisol modified with both Aroclor 1254 and dioctyl phthalate was also more resistant to 25 percent chromic oxide at 50C for four weeks and was equivalent at 23C for six months in comparison with the dioctyl phthalate-modified vinyl plastisol.
TradWMffc of Gdo Chnkcal Co.
DSW 379651
STLCOPCB4100423
Migration Resistance
The use of Aroclor 1262 as a coplasticizer with dioctyl phthalate greatly enhances the resistance of plasticizer migration to nitrocellulose lacquers and films. Table 3 compares this property for four formulations.
TABLE 3
PLASTICIZER MIGRATION TO NITROCELLULOSE LACQUERS AND FILMS
Plasticizer*
Dioctyl Phthalate Polymeric Plasticizer Aroclor 1262 Hardness. Shore "A"
Time (weeks) Room Temperature
1 2 3
Aroclor and OOP (parts)
66
--
20 72
No Change No Change No Change
4 No Change
5 No Change
10 No Change
50 C 1 No Change
2 No Change
3 No Change
4 No Change
5 No Change
10 No Change
General Motors Lacquer Indentation,
Test (158*F; 72 hr.; Very Slight
M-psi load)
Softening
Control OOP (parts)
71 --
--
72
Aroclor, OOP, and Polymeric (parts)1
36
33 20
72
Polymeric and DOP (parts)
38 35
--
73
No Change No Change No Change
No Change
No Change
No Change
No Change
No Change
Very Slight Marking
Very Slight Marking
Very Slight Marking
Very Slight Marking
Slight Marking Slight Marking Slight Marking
Slight Marking
Slight Marking
Slight Marking
Slight Marking
Slight Marking
Slight Marking
Moderate Marking Moderate Marking Moderate Marking Extreme Softening
Moderate Marking
Severe Marking
Very Slight Softening
Slight Softening
Slight Softening
Slight Softening
Lifting
Very Slight Softening
Very Slight Softening
Slight Softening
Slight Softening
Slight Softening
Moderate Softening
Extreme Softening
a) Formulation
Ingredients
Opalon 660 PVC Resin Epoxy Soybean Oil Barium-Cadmium Laurate Calcium Carbonate Plasticizer
Parts by Weight
100 3 3 25
as indicated
osfi
9
STLCOPCB4100424
P/astiso/s
The use of an Aroclor as a coplasticizer with dioctyl phthalate in polyvinyl chloride plastisols or organosols contributes greatly to the viscosity stability Of these materials, especially at elevated tempera tures. This benefit is especially important whenever shelf stability is required. Although the initial viscosity of the plastisol or organosol is increased by the use of an Aroclor in the formulation, the viscosity reduction upon temperature elevation (before the fusion temperature is reached) is much greater than when most other plasticizers are used.
A comparison of the viscosity stability of plastisol formulations with and without Aroclor is given in Table 4.
TABLE 4
VISCOSITY STABILITY OF PLASTISOLS
Dioctyl Phthalate
(80 phr) Viscosity
(poises)
Aroclor 1254 (20 phr)
Dioctyl Phthalate (60 phr) Viscosity
(poises)
25C Initial
1 Day 1 Week 2 Weeks
4 Weeks
36 65 97 116 132
49 63 78 75 148
40C Initial
1 Day 1 Week
2 Weeks
4 Weeks
37 84 215 305 426
48 98 108 110 209
50C Initial
1 Day
1 Week
2 Weeks
4 Weeks
66 gel
94 660 980 gel
a) Brookfield LVF viscometer. No. 4 spindle. 12 rpm
Aroclor 5480 (20 phr) Dioctyl Phthalate (60 phr)
Viscosity` (poises)
92 154 161 178 252
68 136 139 164 274
100 470 900 gel
Dipping Plastisols. The chemical resistance of Aroclor compounds is used to good advantage in chrome-plating-bath coatings and in glove coatings, as illustrated by the following formulation for a clear glove dipping plastisol:
Ingredients Opalon 440 PVC resin Aroclor 1254 Diisodecyl Phthalate Santicizer 160 HB-40 Secondary Plasticizer Liquid Barium-Cadmium Stabilizer Liquid Chelator-Stabilizer Santocel 54 Silica Aerogel
Parts by Weight 100 20 50 25 20 2 0.5 3
SW 379653
STLCOPCB4100425
Sealers. The adhesion-imparting characteristics of Aroclor compounds, their oxidation stability, and their chemical resistance are utilized in the manufacture of automotive sealers, such as the following suggested starting formulations:
Ingredients
Parts by Weight
Opalon 440 PVC resin Vinylite' VMCH resin Aroclor 1260 Diisodecyl Phthalate Santicizer 160 Calcium Carbonate Epoxy Soybean Oil Dibasic Lead Phosphite
96 4 50 100 28 125 5 3
Fabric-Coating Vinyl Dispersions. The use of Aroclor plasticizers in organosol or plastisol formulations enables the manufacture of fireretardant free films and coated fabrics with a high degree of hardness, yet flexibility. The following typical starting formulation for a vinyl organosol to be used for free film or coated fabric illustrates this effect:
Ingredients
Parts by Weight
Opalon 440 PVC resin Dioctyl Phthalate Aroclor 1254 Liquid Barium-Cadmium Stabilizer Epoxy Soybean Oil Thinner Xylene
100 33 10 2.5 3 20-35 15-25
Rigid Plastisols. The viscosity characteristics of the Aroclor plasti cizers are utilized in the following formulation for rigid, rotationallycast objects. The formulation is very viscous when first made up, but when heat is applied, the viscosity decreases so that a smoothly-flowing plastisol is obtained. The finished object has a Shore "D" hardness of 63.
Ingredients
Parts by Weight
Opalon 440 PVC resin Geon" 202 PVC resin Aroclor 1254 Santicizer 141 Epoxy Octyl Tallate Liquid Barium-Cadmium Stabilizer Liquid Zinc Stabilizer Polyethylene Glycol 400 Monolaurate
55 45 35 10 5 2 0.5 1
Tfidomork of Union CarfeMo Corp. **Tntftmrk of B. F. Goodrich Chotnksl Co.
DSW 379654
Vinyl Foam
Aroclor 1262 and 1268 impart fine, uniform cell structure and flame resistance to chemically-blown vinyl foam, as shown by the following formulations:
Ingredients______________________ Parts by Weight
Opalon 440 PVC resin
100 100 100
Aroclor 1262
-- 20
--
Aroclor 1268
20 -- 10
Dioctyl Phthalate
40 -- --
Diisodecyl Phthalate
-- 50 30
0i-(/7-0ctyl. /7-Decyl) Adipate
-- 10 30
Santicizer 214
-- 15 --
Santicizer 409
50 -- --
Butyl Oleate
5 ----
Liquid Barium-Cadmium Stabilizer
233
Epoxy Resin
--22
Neutral Calcium Petronate
3.6 3.6 3.6
Calcium Oxide
--1
1
Sodium Lauryl Sulfate
-- 1.6 1.6
Nitrosan* Chemical blowing agent 10 10
5
Flame-Retardant Floor Tile
The nonflammability of the Aroclor compounds suggests their use in the manufacture of flame-retardant vinyl-asbestos floor tile for military applications. In Table 5 is presented an evaluation of three Aroclor plasticizers in typical vinyl-asbestos-tile formulations. Substitution of antimony oxide for part of the limestone is suggested for still greater fire retardance.
TABLE 5
EVALUATION OF AROCLOR IN FLAME-RETARDANT. VINYL-ASBESTOS FLOOR TILE
Santicizer 160 Aroclor 1254
Aroclor 1260 Aroclor 5460
McBurney Inden tation Hardness Banbury Time (to reach 280'F, sec.) Time to band on roll mill (sec.) Plasticity
Tack Surface a) Formulation
Control (parts)
37
--
--
-- 7.8
99
15
Excellent Excellent Excellent
Aroclor 1254 (parts) 30 15
--
-- 9.6
96
10
Excellent Excellent
Fair
Aroclor 1260 (parts) 36
--
17 -- 10.4
102
10
Excellent Excellent Excellent
Aroclor 5460 (parts) 40
--
--
20 11.2
115
5
Excellent Excellent Excellent
Tndw--rfcof L I. d Pont to Namown t Co, Inc.
DSW 379655
STLCOPCB4100427
In Polyvinyl Acetate
ingredients
Opalon 506 PVC Resin
Santicizer 160
-
Aroclor
Asbestos
Limestone
Titanium Dioxide
Stabilizer
Parts by Weight-
100 As Indicated As Indicated
160 290 15
5
Aroclor compounds are excellent plasticizers for polyvinyl acetateemulsion adhesives and hot-melt adhesives. The excellent tack and strong bonding power they impart and their low cost contribute greatly to the performance and profitability of these adhesives.
Emulsion Adhesives
The liquid Aroclors -- such as Aroclor 1221, 1232, and 1242 -- blend readily by simple stirring with polyvinyl acetate emulsion at up to 11 parts per 100 parts of emulsion. They greatly improve the quick-tack and fiber-tear properties of the adhesive. The performance of Aroclor plasticizers in polyvinyl acetate-emulsion adhesives is compared with that imparted by dibutyl phthalate in Table 6. The following is suggested as a typical starting formulation for a low-cost, quick-tack adhesive:
Ingredients_________________________ Parts by Weight__________
Geiva S-55 PVAc Emulsion100
Aroclor 1232
11
TABLE 6
PERFORMANCE OF PLASTICIZERS IN POLYVINYL ACETATE-EMULSION ADHESIVES
Hardness (Shore "A")
Low- Temperature Flexibility (Clash & Berg. If. C)
Dibutyl Phthalate (11 phr)
69
-10.2
Aroclor 1221
(11 phr) 66
-5.9
Aroclor 1232
(11 phr) 86
4.0
Aroclor 1242
(11 phr) 97
5.3
Volatility (24 hr., 86"C over activated charcoal) 4.0 4.8 (Plasticizer lost, %)
Kerosene Extraction (24 hr.. 25C)
(Plasticizer lost %)
4.1 4.5
Formulation Viscosity (cp.) Initial'
2420
2240
1 Day
2460
--.
3 Days
-- 2200
4 Days
2520 --
5 Days
-- 2200
7 Days
-- 2180
10 Days
-- 2260
a) Initial viscosity of unplasticized emulsion: 1500 centipoises
4.3
3.8
2160
--
2060
--
2040 2020 2060
4.0
4.2
_
-- -- -- --
DSW 379656
STLCOPCB4100428
In Ethylene Vinyl Acetate
When the slight odor of Aroclor is objectionable in an adhesive for certain applications, it can be easily masked, at negligible cost, by the addition of a small amount of Santomask II.
Hot-Melt Adhesives
Aroclor compounds are widely used as plasticizers in polyvinyl acetate hot-melt adhesives for bookbinding and other applications. Four sug gested started formulations for evaluation are as follows:
Ingredient
Parts by Weight
Polyvinyl Acetate Opalon 505 PVC resin
Application Temperature 165- 175C
95' 100-
5--
LowMelting
50*
--
AlkaliDispersable
38'
--
Modified Rosin Coumarone-lndene Resin (soft) Aroclor 1254
----
----
-- 55
25
--
12
--
28.3 27
Aroclor 1260 Dibutyl Phthalate
50-75
--
-- --
--
13
--
7
Santicizer 160 (or dibutyl phthalate) 50-75 30
--
--
Clay
-- 25
--
--
Fluxing Resin (Filtros Resin WW) --
75
--
--
Acrawax C*
----
--
1
Sodium Benzoate
----
--
0.76
Viscosity (centipoises)
2000 (120C) Non-blocking
3500 (175C) Non-blocking
a) Gelva V-7 bj Gelva C-3 V-10 c) Gelva C-5 V-16
The Aroclor products are among the most compatible, effective, and versatile plasticizer/modifiers available for ethylene vinyl acetate. Both the liquid and solid Aroclor plasticizers are highly compatible with ethylene vinyl acetate and other ingredients commonly used in ethylene vinyl acetate, such as paraffin and microcrystalline waxes and other resin modifiers. Aroclor offers special functional properties and reduces formulation costs when used with ethylene vinyl acetate.
Hot-Melt Adhesives
Aroclor in ethylene vinyl acetate hot melts imparts excellent initial tack and high final bond strength. Aroclor is particularly useful in providing versatility of adhesive bond to various substrates such as aluminum foil, cellophane, polyethylene, Mylar** polyester film and paper. Liquid Aroclor, such as Aroclor 1254, provide greater flexibility and lower application viscosities. Solid Aroclor 5460 provides adhesive strength, permanence, and lowers the melt viscosity. Both liquid and solid Aroclor products are exceptionally heat stable, resistant to oxidation, moisture, and chemical attack and are, in general, very inert. Flexibility, specific adhesion, and melt viscosity may be adjusted by varying Aroclor concentration and by selection of solid and/or liquid Aroclor plasticizers. "Trademark of Glyca Chemicals. `"Trademark of DuPont Co.
DSW 379657
STLCOPCB4100429
In Epoxy Resins
Pressure-Sensitive Adhesives
Aroclor in ethylene vinyl acetate pressure-sensitive adhesives imparts excellent specific adhesion and tack. Liquid Aroclor, such as Aroclor 1248 or 1254, improve flexibility and adhesion while solid Aroclor 5460 or 5442 impart a high degree of tack and bond strength.
Suggested starting point formulations for evaluation using Aroclor in
ethylene vinyl acetate hot-melt and pressure-sensitive adhesives are shown below:
Hot-Melt Adhesive
Pressure-Sensitive Adhesive
Parts by Weight_________________
Parts by Weight
"Elvax"'
40 "Eivax" 150
30
Aroclor 5460 40 Aroclor 5460
40
Microcrystalline Wax
20
Aroclor 1254
50
The Aroclor plasticizers probably have greater compatibility with epoxy resins than any other available nonreactive plasticizer-modifiers. The excellent chemical resistance, oxidation resistance, and adhesive qualities imparted by the Aroclor compounds reinforce these important beneficial properties of epoxies and thereby help the compounder reduce his formulation costs materially without significant adverse affect on performance.
The lower-molecular-weight, liquid Aroclor plasticizers (such as 1221 and 1232) have maximum plasticizing efficiency and impart the most flexibility to epoxy compounds. The more viscous, resinous Aroclor products have progressively less effect on epoxy flexibility: the highmolecular-weight, solid Aroclor plasticizers (1268, 2565, 4465, 5460, etc.), in fact, tend to reinforce the compound.
The effects of Aroclor 1221 and 1248 on the properties and performance of an epoxy resin are indicated by the data in Table 7.
TABLE 7
EFFECT OF AROCLOR 1221 AND 1248 ON PROPERTIES OF EPOXY RESINS
Formulation*
Viscosity*
Physical Properties
Physical Property* After Heat Aging
Izod Clarity Before After Impact (Light Hardness Hardness Weight Aroclor Aroclor Curing Curing Resist Reflect Shore "D" Shore "O" Loss 1221 1248 Agent Agent ance ed) (%) (10 sec.) (10 sec.) (%)
-- -- 12.800 7900 0:2 3.0 (30 rpm)
76
86 0.012
25 -- 1650 1200 - 3.0 -- 25 7700 4300 0.6 3.0
8 40
81 2.118 88 0.682
*Tr4*mark of Do Pont Co.
DSW 379658
15
STLCOPCB4100430
Ingredients
Parts by Weight
a) Liquid Epoxy Resin
100
Tetraethylenepentamine
8
Aroclor 1221 or 1248
As Indicated
Cure: 30 minutes at 100C
b) Brookfield LVF No. 4 spindle; 60 rpm unless otherwise specified
c) 24 hours at 86C in activated charcoal
Development of flame-retardant epoxy resins is of wide-spread interest. Aliphatic amine-cured epoxy-resin formulations are made self extinguish ing by the use of 20 parts of liquid Aroclor per hundred parts of resin. The incorporation of antimony oxide at 5 phr, with 15 parts of Aroclor per hundred parts of resin, yields nonburning formulations (Table 8).
The use of liquid Aroclor in aliphatic amine-cured epoxies also improves flexural strength and compressive-yield strength, has little effect on tensile strength, and slightly lowers heat-distortion temperature and compressive ultimate strength.
The use of solid Aroclor in phthalic anhydride-cured epoxy systems also reduces flammability and, in combination with antimony oxide, produces nonbuming formulations. The solid Aroclor products also greatly improve such important properties as compressive strength, flexural strength, compressive-yield strength, and tensile strength, although they slightly lower the heat-distortion temperature (Table 9.)
Extension of epoxy-resin adhesives with Aroclor greatly reduces the formulation cost, with minimum effect on the bonding characteristic of the adhesive or surface coating.
In epoxy-resin protective surface coatings, the use of Aroclor 1254, 1260, or 1262 economically imparts excellent chemical resistance, particularly to acids and alkalies. When resistance to solvents is de sired, however, Aroclors should not be used, since they are true plasti cizers and do not combine chemically with the epoxy resin. Frequently, about 10 to 15 per cent Aroclor 1260 or 1262 is added to increase the flexibility of the epoxy composition, with minimum effect on the corrosion resistance and adhesion of the film.
DSW 379659
STLCOPCB4100431
a
ll*
s; ft
0C3 i.,g^* -5&>-^v. ! s 1^ ^ 'E;j
-S? 'i5
It1 lS J~ '
" 12 Sjj' -
<.|tL |g i =*=c.$a 1
fC-' 03 CO -S.
$ C5
^a 3 ^ I it S"g
5.-S a .C-*j <=3
803 :.
=fsil
I*
{it
u5 g5P .fe t*
.^5f3t ^C^\,3---fe-v
a s>
CD o <=3 o CO CD o C=3 <=> CD
t s; a-a- LC5 r-*
r-
co CO
CO t=>
<3 <o CM CO
CO ^a-
CD o CD o o
C=> o CD o o
05 CO G> LO CM
1.21^: CD cm"
o r_
<3 Sj
CM CM CM CM CM
CD CD O o O
I !". CD o CD CD o O CO LO t-- CM *--? CO r-T r-' C>
CD o O CD o
CD CD t=5 O CD
a ? 05 05 CO O o CO LO CO o 05
"*- o
CM CM CM
. .
LO
g o l"p CO CO LO
LO
*a* CM CO CO CO
<=a
<5
.CD) *o TD
03 +03*
CO co o LO o u u
o r-
*5 a
C/)
c
c --
CO CO
co CO <0
<50 -fSt |e<34-'--s
co o
CO CO
o
CO co
<=>
5:
*o
<<0o ^'
1|03 ^ CO CM CO CM
^ti
C- BV3 it 1 1 1 LO LO
CD
CD
o LO
co
c 03
I"C
1
vj
a
2S
-s3P-
1
1 C5 CM
1 LO
to "O 03 05 cc "O
CO LO >- 03 CO o "O
CO CO
T--55
.03 a
> _d Xc o< a. LU o
CO u <55
CO CO CM
X o
a 0 _c
> c
0
SCO'S-
a To o>
CT *-->
oo
CJ E
o
'4--' c
03 O
1 o [ LO |
_l Q_
<<O
SX
CM
"eo"
DSW 379660
17
STLC0PCB4100432
In Polyester Resins
18
The highly chlorinated, less-volatile Aroclor compounds such as Aroclor 1260, 4465, and 5460, are very effective and economical fire retardants for polyester resins, and they do not significantly affect the physical properties of the resin.
The Aroclor plasticizers are effectively used in combination with equal amounts of antimony oxide, since the two materials are synergistic: Aroclor imparts self-extinguishing properties to the resin, and antimony oxide reduces afterglow.
Table 10 indicates the degree of flame resistance imparted to a generalpurpose polyester resin (with a 35 percent styrene content) by various equal concentrations of antimony oxide and one of these three Aroclor plasticizers.
TABLE 10
FIRE RETARDANCE IMPARTED TO POLYESTER RESINS BY AROCLOR AND ANTIMONY OXIDE
Antimony8 Oxide and Aroclor
1260
2.5% --
4465 --
5460 flammable
a) Formulation
5% semiflammable
flammable
self extinguishing 60 seconds
7.5% semiflammable
self extinguishing
5 seconds
~
10%
self extinguishing 30 seconds
self extinguishing
5 seconds
self extinguishing
5 seconds
15%
self extinguishing immediate'
self extinguishing immediate
self extinguishing immediate
Ingredients Polyester Resin (general purpose) Styrene Methyl Ethyl Ketone Peroxide
(60% in dibutyl phthalate) Cobalt Naphthenate (1% solution) Aroclor and Antimony Oxide
Weight Percent 62 35
2 1 as indicated
Inclusion of an Aroclor increases the flexural strength of the naturally
brittle polyester and makes addition of a more expensive plasticizing
polyester unnecessary. At a concentration of 10 percent (enough for
fire retardancy), none of the Aroclor plasticizers reduced the flexural
strength of the cure resin significantly (Table 11), and their effect was
comparable to that of a plasticizing polyester. At 20 percent addition,
they improved the impact strength, whereas the plasticizing polyester
reduced it. The solid Aroclor plasticizers are preferred for fire-resistant
surface coatings.
i
DSW 379661
<S
STLCOPCB4100433
In Polyethylene In Polystyrene
TABLE 11
EFFECT OF AROCLOR ON STRENGTH OF FIBER-GLASS-REINFORCED POLYESTER RESINS
Plasticizer
Flexural
Strength (%) (psi)
None 0 47,210
Plasticizing Polyester
10 20
43,310 39,930
Aroclor 1260
10 45.600 20 33,880
Aroclor 4465
10 40,740 20 33,390
Aroclor 5460
10 37,400 20 35,890
Flexural Modulus
(psi)
2,190,000
2.000,000 1.560,000
2,090,000 1.690.000
2.190,000 1,290,000
1.700,000 1,550.000
Impact Strength (ft.-lb.lin.)
1.73
1.64 1.24
1.33 2.04
1.41 2.48
1.85 3.06
The need to make polyethylene and other polyolefins flame retardant is well recognized. The well-known flame retardancy of the Aroclor products suggests their evaluation for polyolefin applications such as molded products, coatings, and hot-melt adhesives.
Preliminary evaluation of Aroclor 5460 (20 percent) and antimony oxide (10 percent) showed good results in imparting flame retardancy to low-density, noncrystalline polyethylene. Compared to the use of chlorinated aliphatic hydrocarbons, the use of Aroclor greatly improved the heat stability and had considerably less effect on tensile strength, yield, and elongation of the formulation.
The Aroclor products are good plasticizers for polystyrene. The lowermolecular-weight Aroclor plasticizers have greater solvating power than the higher-molecular-weight Aroclor products. The gelling rate of various plasticizers in polystyrene resin is shown in Table 12, each plasticizer was added to the polystyrene resin at a concentration of 2 parts plasticizer per part of resin, and the time required for the material to gel was noted.
TABLE 12
GELLING RATE OF PLASTICIZERS IN POLYSTYRENE
Plasticizer (200 phr)
Aroclor 1221 Diethyl Phthalate Dimethyl Phthalate Aroclor 1242 Santicizer 141 Santicizer 160 Santicizer B-16 HB-40
Time to Gel (min.)
immediate 0.6 0.75 2 3 6 18 30
DS\N 379662
1
STLCOPCB4100434
In Polyurethanes
20
Aroclor products are useful as plasticizers and flame retardants in polyurethane rubbers, foams, adhesives and coatings. Having extremely low moisture content (50 ppm or less), the Aroclor plasticizers are useful in applications where low moisture is required. Other advantages exhibited by Aroclor in polyurethanes include resistance to oxidation, resistance to alkali and acids, improved adhesion, and low cost. The following formulation illustrates the use of Aroclor 1254 in a polyure thane flocking adhesive:
Part A Part B
ingredients Muitranii' FLD Urethane Resin Mondur' C Isocyanate Aroclor 1254 Muitranii FLD Mondur C
Parts by Weight 100 5 20 100 5-10
Part A is applied to the fabric by knife coating and allowed to dry thoroughly. The fabric is then coated with Part B, and the material is flocked immediately.
Protective urethane coatings are unusually well suited for application to concrete and metal. Aroclor 1254 is incorporated to improve ad hesion and sealing. The first of the following formulations is the preferred prime coat for concrete storage tanks for gasoline and fuel oils. The second formulation is the base coat for a concrete wood-kiln coating, which remained in perfect condition after two-and-one-halfyears' continuous exposure to heat, moisture, and wood distillates. The other two formulations, for primer and intermediate light-metal coating, contain Aroclor 1254 for better adhesion to metal.
Ingredients Mondur C Muitron R-4 Polyester Resin Muitron R-10 Aroclor 1254 Polyvinyl Acetate Polyvinyl Butyral Methyl Glycol Acetate Butyl Acetate Ethyl Acetate Toluene Pigment (colored) Zinc Chromate Titanium Dioxide (rutile) Talc (micronized)
UnsealedConcrete Prime Coat (parts)
19.0
-- 10.0 5.0 0.2
-- 8.7 8.7 8.7 8.7
12.5
-- -- 12.5
HighTemperature
Concrete Primer (parts)
12.0
12.0
2.9
-- 0.4
9.0
5.4 4.0
6.9
--
-- 15.0
13.9
Light-Metal Coating
Primer Intermediate
(parts)
(parts)
21.0 25.1
2.6 7.2
10.5 7.2
2.7 1.8
0.3 0.3
----
----
8.0 7.5
8.0 7.5
15.1 14.2
6.7 21.0
7.9 --
----
13.2 5.5
`Muitranii and Mondur: Mobay Chtmteal Company trademarks.
DSW 379663
1
STLCOPCB4100435
In Phenolic Resins
Considerable interest has been shown in the use of Aroclor plasticizers to make phenolic laminating resins flame retardant. The highermolecular-weight Aroclor products (1262 and 5460) are usually evalu ated for this purpose.
Aroclor 1268 and 2565 are useful in the manufacture of brake linings.
A
Chlorinated rubber primer and topcoat, plasticized with Aroclor, offer excellent resistance to outdoor weathering, high humidity, steam and condensed acid vapors.
Aroclor In Rubbers
In Chlorinated Rubber And Chlorinated Polypropylene
Protective coatings based on chlorinated rubber generally contain Aroclor plasticizers to enhance their chemical resistance (to water, alkali, and acid), corrosion resistance, and electrical insulating proper ties and to impart flame retardance. When properly pigmented, they are unusually weather resistant. Aroclor compounds strengthen the adhesive grip of chlorinated-rubber lacquers, varnishes, and paints to structural materials and improve the flexibility and life of the coating.
Typical applications include protective and decorative coatings for swimming pools, stucco homes, steel structures, tank cars, and both wood and metal maritime equipment. Their outstanding chemical resistance qualifies these coatings for use in manufacturing plants where chemical attack is prevalent. Aroclor 1254 and 1260 are used in chlorinated-rubber coatings as flexibilizing plasticizers, commonly in combination with Aroclor 5460, which serves as a resin fortifier. A variety of suggested starting formulations based on chlorinated rubber is given in the following table.
DSW 379664
21
STLCOPCB4100436
Paints for Alkaline Surfaces
Ingredients
Fed. Spec. TT-P-91 (parts)
Concrete Swimming
Pool
(parts)
Maximum Acid and Alkali
Resistance
(parts)
Parton' (20 cp.) Chlorinated Rubber 18
10.2 18
Aroclor 1254
10 5.1 8
Aroclor 1260
----
6
Aroclor 5460
6--
--
Long-oil. oxidizing, alkyd resin
----
-
Medium-oil, drying, alkyd resin -- 5.1
--
Carbon Black
0.5 --
--
Iron Oxide
----
18
Titanium Dioxide
16 11.4
-
Zinc Oxide
2--
--
Asbestine" 3X (magnesium silicate) --
11.7
--
Bentone'" 34 gelling agent
-- 1.3
--
Epichlorohydrin
-- 0.1
0.09
Stabilizer
----
0.9
So/vesso"" 150
42.75 --
--
So/vesso 100
-- 9.1 45
Turpentine
4.75 --
5
Xylene
-- 45.7
-
Hi-Flash Naphtha
----
-
White Marine Paint (parts)
20 6 -
--
6 -- -- 25 --- -- -
-- 23 20
Aroclor compounds are also incorporated in chlorinated-rubber for mulations used for heat-sealing adhesives, electrical coatings, paper and textile coatings, and printing inks. The following starting formula tion is for an acid- and flame-resistant adhesive:
Ingredients
Chlorinated Rubber (125-cp. type) Aroclor 1254 Aroclor 5460 Toluene
Parts by Weight
20 6 6 68
Chlorinated polypropylene, a new film-forming resin, produces clear, colorless films, appears equal to chlorinated natural rubber in chemical resistance, and is noticeably more heat and light stable. Aroclor is very compatible with the resin and is recommended in the following start ing formulations:
Ingredients Chlorinated Polypropylene Aroclor 5460 Aroclor 1254 Dioctyl Sebacate Epoxy stabilizer Solids, wt. percent in toluene
Composition (wt. %)
50.0' 55.0A 15.0 15.0 24.0 24.0 4.3 4.3 1.7 1.7 50.0 " 50.0
'Trademark of Hercules Inc. 'Trademark ot International Talc Co. "Trademark of National Lead Company "'Trademark of Standard Oil Company (N. J.)
DSW 379665
STLC0PCB4100437
300Fbeat stability 1 hour 2 hours 3 hours 5 hours 18 hours
Film Properties
v. si. yellow v. si. yellow si. yellow mod. yellow black
v. si. yellow si. yellow mod. yellow
--
--
Fade-Ometer* stability 24 hours 48 hours 96 hours 144 hours
si. yellow si. yellow mod. yellow mod. yellow
v. si. yellow si. yellow si. yellow brown
Two-neek chemical resistance water 10% hydrochloric acid 1% sodium hydroxide
excellent excellent excellent
excellent excellent excellent
a) Parlon P (10-cp, 20% in toluene) -- Hercules Inc.
b) Parlon P (20-cp. 20% in toluene) -- Hercules Inc.
c) Lacquers were sprayed on "bonderized" steel panels. Films were 2.5- to 3.0-mils thick after 72-hours' air drying.
|n Styrene-Butadiene Copolymers
Aroclor plasticizers are very often incorporated in coatings based on styrene-butadiene copolymers to impart resistance to acids, alkalies, moisture, and corrosive chemicals. These coatings are suited for use on masonry, wood, and metal for such applications as concrete floors; architectural finishes; metal primers and finishes on maritime equip ment, structures, and tank cars; baking primers; corrosion-resistant industrial films; and oil- and grease-resistant coatings.
The following suggested formulations for typical applications of
styrene - butadiene - copolymer coatings offer excellent performance:
Ingredient
Clear Wait Aluminum
Traffic
Vehicle Sealer Enamel Paint Paint
(wt. %) (lb.1100 gal.) (wt. %J (lb.) (parts)
Styrene-Butadiene
16.60s 123.2*
7.40s 147rf 250s
Aroclor 1254
8.39 41.4 6.00 - 120'
Aroclor 1260
-- -- -- 31 -
Aroclor 5460
9.11 41.4 13.40 - 130
Raw Tung Oil
1.655 --
-- ----
Hydrogenated Methyl Abietate
--
--
--
8-
Troykyd" ABC
------
3-
Lecithin
0.545 --
-- ----
Soya Lecithin
--
5.9 --
----
Petroleum Naphtha
62.70 246.4
--
----
Hi-Flash Naphtha
-- -- -- 395 -
Mineral Spirits No. 10
-- 185.3 33.60 - 340
Toluene
-- -- -- - 340
Xylene
-- -- 22.40 -- --
'Trademark of Atlas Electric Devices Co. ''Trademark of Troy Chemical Co.
;
DSW 379666
STLCOPCB4100438
Lithopone Titanium Dioxide Aluminum Stearate Aluminum Paste Zinc Oxide Barium Sulfate Asbestine 3X (magnesium silicate) Calcium Carbonate, ground Diatomaceous Earth Mica
-- -- -- -- -- -- -- -- -- --
339.3 59.2 5.9
--
--
--
75.0 -- -- --
---- -- 179
----
8.55 -- -- 60 -- 90 ---- -- 236 -- 76 8.00 30
a) Marion "9200" MV (Trademark of Marbon Chemical Div., Borg-Warner Corp.)
b) Pliolite S-5A (Trademark of Goodyear Tire and Rubber Company)
c) Marbon "9200" LV (Marbon Chemical Div., Borg-Warner Corp.)
dj Flaked Piccofle,r 120 (Trademark of Pennsylvania Industrial Chemical Corp.)
e) Pliolite S-5B (Goodyear Tire and Rubber Company)
fj or Aroclor 1248
--
--
--
--
--
-- -- -- --
--
In Synthetic And Natural Rubbers
The liquid Aroclor plasticizers -- 1221,1232, 1242, and 1248 -- have a strong plasticizing action on both natural and synthetic rubbers. Solid Aroclor -- 1254 and 1260 -- imparts permanent tackiness and adhesion to the rubber composition.
Neoprene
Compositions containing up to 40 parts of Aroclor 5460, 2565, 4465, or 1268 in 100 parts of neoprene rubber are extremely fire retardant. About 1.5 parts of Aroclor 1268 per hundred parts of neoprene imparts excellent working qualities at 225 to 325 F for injection moldings. Neoprene modified with Aroclor compounds has proved extremely useful as a wire and cable coating.
Aroclor 5460 imparts plasticization and adhesion to decorative and protective coatings that have been commercially used on rubber products for many years. Suggested starting formulations for a clear, dull coating and for three pigmented coatings are as follows:
Ingredients
Aroclor 5460 Neoprene GRN-10 Chlorinated rubber (21 cps.) High-styrene resin Isobutyl methacrylate Toluene
Parts by Weight
dear, dull coating
base for pigmented coatings
3.70 16.00
3.50 8.00
1.30 --
1.00 4.38
0.40 1.75
90.10 69.87
DSW 379667
STLCOPCB4100439
Ingredients Paste:
Base Chromium Oxide Zinc Oxide No. 3 Titanium Dioxide Aluminum Hydrate Toluene
green coating
20.0 6.4 3.6 -- -- 10.0
white (high gloss)
white {luster modifier}'
43.0 29.0 ---- 10.5 -- 15.0 -- -- 25.0 31.5 52.0
Ready-to-Use Coating:
Base Paste
60.0 70.0 40.0 30.0
*To modify the luster of the white, high-gloss coating, the selected amount of the modifier composition is in corporated into the high-gloss paste to achieve the desired degree of flatness.
Polybutene
Aroclor plasticizers and Indopol* polybutenes are blended in various proportions to make permanently tacky coatings for fabric or paper. Insecticides, for example, can be blended into such coatings to make insect traps or barriers on tree trunks for foliage or fruit protection. Such coatings can also be used for tape and sign backing.
Excellent sealing and caulking compounds are made with blends of Aroclor and polybutenes with inorganic fillers, such as:
ingredient Whiting Talc Lithopone Asbestos
Percent 50 30 10 10
By various combinations of selected Aroclor compounds and poly butenes, a wide range of hardness, viscosity, flow, and bonding charac teristics can be produced in durable sealing and caulking compounds.
Specialty mastics, too, are obtained by selective blends of Aroclor plasticizers with polybutenes. They have excellent adhesivity for such uses as automobile-body sealants.
*Trsdtmifk of Amoco Chomicals Corp.
DSW 379668
25
STLCOPCB4100440
Paper-transparentizing liquids (for making tracing paper, window envelopes, and special packaging) can be formulated with Aroclor 5460 and polybutenes. A typical economical formulation is as follows:
ingredient
Percent
Aroclor 5460
30
Polybutene (Indopol H-300)
25
Toluene
45
Butadiene-Acrylonitrile Rubber The Aroclor plasticizers -- particularly Aroclor 5460 -- are useful as softeners for Buna N rubber.
Silicone Rubber Aroclor is a very effective flame retardant for silicone rubbers.
Crepe Rubber (Natural) Aroclor 1262 is used as a low-cost plasticizer for crepe rubber in paint compositions. In concentrations of from 5 to 50 per cent of the weight of the rubber, the Aroclor increases the films alkali resistance, and adhesivity to steel.
Polysulfide Rubber
Aroclor plasticizers are widely used to flexibilize, improve the bond ing strength, increase the chemical resistance, and reduce the cost of Thiokol* polysulfide liquid rubbers. Among the many uses of poly sulfide formulations are joint-sealant compounds used in construction, solvent-resistant gaskets, adhesives for concrete, potting and encap sulation, protective coatings, and binders.
Although the Aroclor plasticizers are highly compatible with poly sulfide rubbers-- up to 100 phr -- the concentration to be used depends on the handling and performance properties required in the finished compounds. Suggested concentrations of Aroclor range from about 15 phr for sealant compounds to about 40 phr for casting formulations.
Liquid Aroclor (such as Aroclor 1248) is used to reduce the viscosity and permit the use of higher filler concentration, whereas the solid Aroclor (such as Aroclor 5460) is useful where low volatility is desired.
The following suggested starting formulations illustrate the use of Aroclor 1232 in a joint sealant compound and of Aroclor 1248 in a polysulfide casting formulation:
Trademark of Thiokol Chemical Corp.
DSW 379669
STLCOPCB4100441
Ingredient Thiokol LP-32 polysulfide Thiokol LP-2 polysulfide Aroclor 1232 Aroclor 1248 Calcium Carbonate Calcined Clay Titanium Dioxide Phenolic Resin Stearic Acid Zinc Sulfide Sulfur C-5 Paste'
Sealant (parts)
100 -- 5-15 -- 20 20 10
5 1 -- 0.1 15
Casting Compound
(parts) -- 100 --
20-40
--
-- --
--
-- 40
0.1 15
Property
Cast sheets, after cure of 7 days at room temperature:
Tensile strength, psi
150-200
Elongation, percent
500-700
Hardness, Shore "A"
30-40
150-200 300-400 25-35
a) lead peroxide, 50%; dibutyl phthalate, 45%; stearic acid, 5%: passed three times through a tight paint mill.
Aroclor In Cellulosic Resins In Ethyl Cellulose
Ethyl cellulose formulations plasticized with Aroclor are used as pro tective lacquers, adhesives, and strippable coatings. The solids, such as Aroclor 5460, are widely used with ethyl cellulose or cellulose acetate-butyrate resins in hot-melt applications for the protection of tools and metal parts.
The Aroclor plasticizers are highly compatible with ethyl cellulose: the liquid Aroclor imparts flexibility; the solids impart hardness. For example, 75 parts of Aroclor 1242 with 100 parts of ethyl cellulose produces a very flexible, slightly tacky material. Aroclor 5460 at the same concentration yields a very hard, somewhat brittle composition. Hard films that contain Aroclor 4465 are not brittle at ordinary temperatures.
For high-gloss coatings with exceptional weathering qualities to be
applied to rigid surfaces, compositions containing equal parts by
weight of Aroclor 5460 and ethyl cellulose are suggested. When a
more flexible coating is required, a softer Aroclor should replace either
all or part of the Aroclor 5460.
'
DSW 379670
27
STLCOPCB4100442
In Nitrocellulose
The following five typical formulations indicate the versatility of various Aroclor plasticizers in compounding for widely different types of applications. They are intended as guides to the use of Aroclor compounds with ethyl cellulose.
Ingredients Ethyl Cellulose Aroclor 1254 Aroclor 1260 Aroclor 5460 Dow 276. V-9 Octylphenol Stearic Acid Rutile Titanium Oxide Epoxy Resin Santonox Antioxidant Mineral Oil Castor Oil Epoxidized Soya Oil Paraffin Wax (m.p. 135FJ
Lacquer (parts)
50 -- 50 -- -- -- -- -- -- -- -- -- -- --
White AlkaliResistant Lacquer (parts)
25 16
-- 76
-- 1
-- 50
1
--
-- --
-- --
Liquid Adhesive (parts)
50 -- -- 40 8 2 -- -- -- -- -- -- -- --
Strippable Coating (parts)
49 49
-- -- -- 1 1
-- -- -- -- -- -- --
Hot-Melt Adhesive
(parts)
24
-- -- 7 -- -- -- -- -- 1 57 5 3 3
The first four of these formulations may be dissolved in suitable solvents, such as mixtures of about four parts of toluene to one part of butanol, to obtain the desired viscosity. .
In nitrocellulose lacquers, the Aroclor compounds can function either as plasticizers to modify the properties of the film or as resin extenders to add film-forming body. They are highly compatible with nitro cellulose and with other resins and plasticizers commonly used in lacquer formulations. They impart weather resistance, luster, adhesion, and flame retardance. Their excellent electrical characteristics and their ability to retard the passage of moisture and gases through nitrocellulose films make the Aroclor compounds especially valuable in coatings for electric-insulating materials.
The following trilinear diagrams (Figure 1), show the limits of practical compatibility of Aroclor 1254, 1260, and 1262 when used in nitro cellulose lacquers in combination with some other resins or plasticizers. The less viscous Aroclor plasticizers (1242 and 1248) are more com patible than those shown; the more resinous Aroclor (1268, 2565, 4465, 5442, and 5460) is less compatible.
In these trilinear diagrams, compositions represented by any point in an unshaded area produce homogenous nitrocellulose-lacquer films. On the other hand, compositions represented by points in the shaded areas produce impractical (segregated, brittle, or soft) films. ;
DSW 379671
STLCOPCB4100443
Fig. 1 -- Limits of Practical Compatibility of Aroclor in Nitrocellulose Lacquers
.0 100-
NITROCELLULOSE, %
50 AROCLOR
1254 or 1262, %
60
100 90 80 70 60 50 40 30 20 10 0
ESTER GUM RESIN, %
NITROCELLULOSE, %
AROCLOR 1260 or 1262, %
100 -X
100 90 80 70 60 50 40 30 20 10 PHTHALIC ANHYDRIDE-GLYCEROL RESIN, %
0
NITROCELLULOSE, %
50 AROCLOR 1254, %
100 90 80 70 60 50 40 30 20 10 PHTHALIC ANHYDRIDE-GLYCEROL RESIN, %
0
DSW 379672
29
STLCOPCB4100444
Fig. 1 (Continued)
?I
0
AROCLOR 1260 or 1262, %
The following formulations are given to illustrate modifications that can be obtained by variations in composition. They all have excellent durability, but the first, two are much harder and less flexible than the third. The first two also have excellent sanding and polishing qualities, but No. 3 is too soft for sanding. The cable lacquer (No. 4) has ex tremely high flexibility, as required for high-tension automobile cables.
DSW 379673 30
STLCOPCB4100445
Ingredient Nitrocellulose ('A sec.) (wet) Nitrocellulose ('A sec.) (dry) Nitrocellulose (15-20 sec.) Aroclor 1242 Aroclor 1260 Aroclor 5460 Dibutyl Phthalate Tricresyl Phosphate Damar Resin Ester Gum
No. 1 (parts)
-- 100 -- -- 20-39 -- 20-0 -- 80
--
No. 2 (parts)
-- 100
--
-- 20 -- 20 -- -- 80
No. 3 (parts)
-- 100
--
--
80-70 -- --
39-70 --
--
No. 4 Cable Lacquer (parts)
-- -- 100 80
--
--
-- 120
--
--
No. 5 Chrome Lacquer (parts)
100
--
--
--
--
47 32.5
--
--
--
In Cellulose Acetate-Butyrate
The high-chlorine-content Aroclor plasticizers are highly compatible with cellulose acetate-butyrate and are widely used in the manufacture of low-cost, flame-resistant lacquers. Typical uses for these products include paper coatings, lacquers for plastics, strippable coatings for paint booths, and hot-melt adhesives. Typical starting formulations, illustrative of these uses, are suggested as follows:
Ingredients
Paper Lacquers
Low-Cost
Flame
Curl
Resistant Resistant
(wt. %)
(wt. %)
Clear Wood Filler (wt. %)
Half-Second Cellulose Acetate-Butyrate
20 20
7
Aroclor 1260
-- 20 --
Aroclor 1262
15 -- --
Aroclor 5460
-- -- 15
Dioctyl Phthalate
----
Epoxy Soybean oii
-- ----
Acrylic Resin
-- ----
Dow 276, V9
-- ----
Socony Vacuum 200
-- ----
"Newport V40"* pine resin
-- ----
Acetone
-- 10 --
Methyl Ethyl Ketone
-- ----
Methyl Osobutyl Ketone
-- ----
Isobutyl Acetate
5 10 22
Ethanol
12 10 --
Butanol
----5
Isobutanol
-- ----
Toluene
48 30
6
Santonox Antioxidant
-- ----
Syn Fleur No. 6 odorant
-- ----
Asbestine X (magnesium silicate)
--
-- 45
a) Coatings for cellophane, cellulose acetate, and cellulose acetate-butyrate.
Plasticsa Lacquer (wt. %)
6 1.5
--
--
--
-- 2.5 1.5 --
--
-- 10 5 -- 33.5 -- 25 15 -- --
--
Paint-Booth Strippable
Coating (wt. %)
20 --
--
9 9 9.5 -- -- 2.5 -- 10 -- -- 5 10 -- -- 25 -- -- --
Hot-Melt Adhesive (wt. %)
35 -- -- 30 15 -- -- -- -- 19.89 -- -- -- -- -- -- -- -- 0.1 0.01 --
Trademark of NwportlndustrisCo.,Oiv.of Heydan NewportChemicalCorp.
SVV 379674
31
STLCOPCB4100446
Aroclor In Paint, Varnish, Wax, Asphalt In Paint And Varnish
Aroclor is soluble in paint and varnish oils and solvents and compatible with most film-forming coating resins. The Aroclor plasticizers improve adhesion to the substrate and impart to the film properties that correspond to the particular character of the Aroclor used: the hard, resinous Aroclor tends to give increased hardness; the viscous Aroclor imparts flexibility.
Aroclor 4465 and 5460 produce paints that are very quick drying and yet have excellent durability. The amount of Aroclor used may be from 30 to 50 percent of the weight of the oils.
Aroclor 1260 is best for short-oil varnishes that are required to be flexible. The Aroclor plasticizers impart water and alkali resistance and also enhance the value of the other resins used in the varnish. A sug gested starting formulation is two parts of oil, one part of Aroclor 1260, and one part of other resin. These proportions can be varied as required. The Aroclor may be considered to play the same role in the varnish formulation as oil, except that it does not oxidize and lose its flexibility on exposure.
The Aroclor plasticizers do not react chemically with oils, hence there is no advantage in heating together in making a varnish. They are best added as a "chill back" or as a cold cut in the thinning operation. The only reason to heat the Aroclor is to fluidize it so that it can be more readily mixed with the oils. Alkyd, phenolic, or ester gum resins, with a harder Aroclor such as 5460, may be used in making varnish formulations. To illustrate the use of Aroclor plasticizers in alkyd resins the following suggested starting formulation is shown.
Ingredients Alkyd (60% Nonvolatile) Kettle Bodied Linseed Oil (Gardner-Holdt Vise. Z-2) Raw Linseed Oil Aroclor 5460 Titanium Dioxide (Rutile) Titanium Dioxide (Anatase) Magnesium Silicate Mineral Spirits Drier-Absorption Agent Penyl Mercury Naphthenate (10% Mercury) Cobalt Naphthenate (6% cobalt) Lead Naphthenate (24% lead) Antiskinning Agent (Volatile type)
Parts by Weight 81 20 35 34 34 67 100 38 1.3 2.7 1.5 3.2 0.67
DSW 379675
i
STLCOPCB4100447
The following suggested starting formulation for a fire-retardant enamel illustrates use of the flame retardancy of an Aroclor in alkyds:
Ingredients 38% Phthalic Anhydride-Soya Alkyd Aroclor 5460 Solution
(Aroclor 5460, 53; Hi-Flash Naphtha, 22) Whiting Colloidal Grinding and Dispersing Agent Antimony Oxide Titanium Dioxide (Rutile)
Parts by Weight 63 75
84 2.7 42 33
Grind above ingredients, and thin with: 38% Phthalic Anhydride-Soya Alkyd Yylene Cobalt Naphthenate (6% cobalt) Manganese Naphthenate (6% manganese) Lead Naphthenate (24% lead)
96 38 1 1 2.3
Aroclor plasticizers are excellent grinding and dispersion media for pigments used in paints and varnishes. Aroclor 1254 is used to disperse aluminum powder in a paste form that can be incorporated easily into paints and varnishes. The Aroclor imparts excellent leafing qualities, brightness, or luster and does not tarnish the aluminum pigment on aging. Moreover, the composition does not support combustion.
Aroclor is an important ingredient of heat-resistant aluminum paints
and enamels that contain silicone resins. For example, the following
suggested formulation for a heat-resistant coating can withstand a
maximum temperature of 800 F and continuous-service temperature
of 400 F. The heat-resistant enamel can withstand temperatures of
900 to 1000 F in such applications as jet-engine components, exhaust
manifolds, and incinerators. The heat-resistant paint has excellent
resistance to a programmed heat test, including 8 hours at 1200 F,
and to salt-water spray after programmed heating to 500, 600, and
900 F.
;
DSW 379676
33
STLCOPCB4100448
In Waxes
"Dow Corning 805"' Resin (50% Nonvolatile)
G E Silicone Resin SR-82 (60% in xylene)
G E Silicone Resin SR-112 . (50% in xylene)
Styrene-Butadiene (50% in xylene) (,P/ioIite S-5B)
Aroclor 4465 (90% nonvolatile)
60% Aroclor Solution (Aroclor 4465, 36 wt. %) (Aroclor 1262, 24 wt. %) (Sotvesso 100, 24 wt. %) (Xylene, 16 wt. %)
Aroclor 5460 (60% in xylene)
Aroclor 1254
Aluminum Paste (74% nonvolatile)
Cobalt Octoate (6% cobalt)
Xylene
Mineral Spirits
a) Meets Spec. TT-P-0028
Heat-Resistant Coating
(ib.HOOgai.) 220 -- --
332
-- -- 384
--
114 --
Heat-Resistant Enamel
(Ib.jlOO ga/.J --
174.2
313.3
--
-- 435.6
-- -- 250.0 4.4 -- --
Heat-Resistant Paint1
(Ib.jlOO gal.) --
93.6
-- 207.9
--
93.6 47.8 240.0
--
140.8 113.1
The Aroclor plasticizers, especially 5460, are compatible with various natural waxes, and are blended with waxes for many uses, including "lost-wax" casting, impregnating compounds, and inexpensive sealers. Waxes formulated with Aroclor are nontacky and stable.
Much of the highest quality precision-casting wax used in the "lostwax" process is formulated with Aroclor, most frequently 5460, 4465, and 1254. Waxes containing Aroclor are widely used in making dental castings, costume jewelry, and precision-cast aircraft parts.
Usually from one-fourth to one-half the composition consists of Aroclor 5460, which contributes these desirable properties to the formulation: hardness without brittleness, shrinkage resistance, sharp definition, sharp melting point, fire resistance, low volatility, and volatilization without carbonization during final curing.
Excellent impregnating compounds to prevent sticking of furniture drawers, double-hung windows, etc. are made from selected Aroclor plasticizers, such as 5460, and various waxes. Combinations of resinous Aroclor with waxes make excellent and inexpensive sealers for masonry, wood, fiberboard, and paper.
Aroclor imparts moisture and gas resistance, adhesion, alkali and chemical resistance, flame resistance, lubricity, and insulation to impregnants for cloth, paper, wood, and asbestos. They are combined with such materials as waxes, asphalt, tars, sulfur, aluminum stearate, and inorganic pigments so as to provide exactly the physical charac teristics required for the specific purpose. Aroclor 1254, 4465, and 5460 are suggested as most applicable.
*Trademarkof OowComlngCorp.
,
DSW 379677
STLCOPCB4100449
In Asphalt In Allyl Starch
Wood is decidedly toughened, hardened, and made more moistureresistant when impregnated by the vacuum-pressure method with the following mixture:
Ingredients Aroclor 4465 Microcrystalline Wax Sulfur
Per Cent 70 20 10
The coating is very resistant to acids and alkalies but can be attacked by aliphatic, aromatic, or chlorinated hydrocarbons. The paintable surface is not appreciably discolored. Various degrees of hardness and adhesion are obtained by variations in the proportions of the ingredients.
Blends of Aroclor 1268 and 1242 have the unusual capability to extend camauba wax satisfactorily and at an attractive saving in cost:
Ingredients Aroclor 1268 Aroclor 1242 Carnauba Wax Ceresin Wax Paraffin Wax
10 5 5 20 60
Parts by Weight
19.6 30
35
4.9 5
5
6.8 10
30
19.6 20
20
49.0 35
10
35 5 50 10 --
Characteristics Color
Texture
Pale Yellow, White
Smooth, hard,
non-tacky
Softening point, C Melting point, C
60 78
Pale Yellow
Smooth, hard,
non-tacky
77 79
Pale Yellow
Smooth, hard, slightly brittle
78
78
Pale Cream
Slight surface crystallinity
79 86
Cream
Smooth; carnauba-
ringed surface
80.5 88
Self-extinguishing asphalt formulations for caulking, roof coatings, and sound-deadening coatings are obtained by incorporation of at least 30 percent Aroclor 5460 or other solid, resinous Aroclor.
Substitution of the hydroxy hydrogen atoms of the starch molecule by allyl groups produces allyl starch, which upon polymerization forms stable, cross-linked molecules. A minimum of 20 weight-percent plasticizer is required to make the film flexible. The aroclor plasticizers are highly compatible and very efficient plasticizers for allyl starch.
DSW 379678
35
STLCOPCB4100450
Miscellaneous Applications Of Aroclor
With their wide range of physical properties, their inertness, lubricity, and low vapor pressures -- Aroclor plasticizers are valuable ingredients in an incredible variety of formulated products. They are compatible with many solvents and oils and most resins. They are virtually non volatile and permanently thermoplastic; they do not react with other chemicals in the formulation. Finally, their low cost makes their use for special purposes eminently practical and economical.
Dust Prevention And Dust Catching
Aroclor 1254 is a low-cost dedusting agent that "holds down" the dusting of a variety of chemical materials. Since Aroclor 1254 resists both oxidation and combustion, it can even be used to control the dusting of highly reactive compounds. As a typical example, a few tenths of a percent controls the dusting of calcium hypochlorite.
Since Aroclor is non drying and tacky, it makes excellent coatings to capture dust, lint, and other fine, airborne particles. Glass fiber, metal mesh, and other materials used to filter air and gas streams are coated with Aroclor 1260 and 5460.
Vapor Suppression (For Longer Insecticide Kill-Life)
The effective kill-life of expensive chlorinated insecticides is extended as much as ten-fold by the incorporation of equal parts of Aroclor 5460, which acts both as a vapor suppressant and as a sticking agent. Hard surfaces (painted or metallic) sprayed with lindane or benzene hexachloride fortified with Aroclor 5460 remain toxic to flies, ants, roaches, and silverfish for as long as three months, compared with one week for unfortified sprays.
The Aroclor retards the rapid evaporation of the volatile insecticides without adding odor or objectionable residue. Formulation into an insecticide is simple: a solution of the Aroclor in a suitable solvent is merely added and mixed into the other ingredients.
Aroclor 5460 is also recommended for noncrop insect formulations containing chlordane, aldrin, and dieldrin. The other resinous Aroclor products (1254, 1260, 1262, 4465, and 5442), also nonvolatile and sticky or tacky, likewise merit evaluation as insecticide extenders.
Moisture Proofing
In moisture-proof coatings for wood, paper, concrete, or brick, Aroclor is best combined with waxes, especially paraffin or carnauba; oils such as mineral oil or drying oils; or synthetic resins, including modified alkyds, phenolics, chlorinated rubber, polystyrene, styrene-butadiene copolymers, ethyl cellulose, cellulose acetobutyrate, benzyl cellulose, or vinyl resins. The material to be used with the Aroclor should be selected according to the end-use requirements of the specific ap plication.
Some very simple compositions contain only Aroclor and paraffin. One very efficient moisture-proofing compound, consisting of 96 weight percent Aroclor 5460 and 4 percent paraffin (melting point 54C.), has
DStV 379679
STLCOPCB4100451
an ASTM softening point of about 82C. A similar compound, based on Aroclor 4465, has a softening point of about 58C.
Softening point and viscosity when melted are further decreased by the use of mixtures of Aroclor. For example, a composition containing 40 percent Aroclor 1260, 56 percent Aroclor 5460, and 4 percent paraffin, is very soft at room temperature. A higher concentration of paraffin also produces softer compounds.
An excellent melt coating for paper and cloth, made according to the following suggested formulation, may be applied by knife or roller at 350F, requires no solvent, and provides an extremely flexible coating.
Ingredients
Half-second Cellulose Acetate-Butyrate Dioctyl Phthalate Aroclor 1260 Santonox antioxidant
Percent 50 9.9 40 0.1
Pigment Dispersion
Aroclor 4465 is a useful resin in rotogravure and other printing inks. It is an important ingredient in the following mimeograph ink suitable for use on bond paper:
Ingredients
Aroclor 4465 Lubricating Oil (SUV 1200 @ 100F) Paraffin Oil (SUV 76 @ 100F) Carbon Black Oil-Soluble Dye
Percent 40 35 20 4 1
Aroclor 4465 is also used in the preparation of imitation gold leaf. Bronze powder is spread upon a hot coating of Aroclor on one side of a sheet of paper. When the paper treated with Aroclor and bronze powder is placed on the object to be imprinted and a hot die is pressed against it, the Aroclor softens, sticks the bronze to the object, and coats the powder to prevent tarnishing.
Aroclor 1254 and 4465 serve as pigment vehicles for decoration of glass and ceramics. When the decorated object is fired, the Aroclor volatilizes without carbonization and thus avoids discoloration. Aroclor plasticizers are also valuable as grinding and dispersing mediums for pigments used in plastics.
Sealing And Impregnation
The liquid Aroclor plasticizers, 1221 and 1254, because of their low vapor pressures and fire resistance, are excellent sealants. These non evaporating fluids have good flow at slightly elevated temperatures and are chemically stable at elevated temperatures. These liquid Aroclor products therefore are excellent fluid seals wherever the use of oil would create a fire hazard. In the trough of annealing furnaces, for example, Aroclor plasticizers are dependable, fire-safe roof sealants.
DSW 379680
3/
STLCOPCB4100452
Because of their nonflammability, high resistivity and dielectric strength, and low power factor, the liquid and resinous Aroclor plasti cizers are extremely valuable impregnants for many electrical applica tions. One important use of Aroclor 1260, 4465, and 5460 is in wire and cable coatings and as impregnants for braided cotton-asbestos insulation. Their high purity and excellent electrical resistance make Aroclor 1254, 5460, and 1268 excellent dielectric sealants: to close the pores of carbon resistors, and to seal electrical bushings and terminals.
Aroclor plasticizers are essential components of coatings for flame proofing cotton drill for outer garments and for rendering olive-drab canvas fire-retardant, water-repellent, and rot-proof for tents, tar paulins, etc., according to the following formulations:
Flameproofing Formula for Cotton Drill
Ingredients
Parts by Weight
(A) Urea-formaldehyde resin monomer
9.62
Catalyst for resin
0.40
Water
22.26
(B) Oil-modified alkyd resin Aroclor 1254 Aroclor 5460 Stoddard solvent
3.89 12.00 14.40 25.15
(C) Antimony oxide, 300 mesh or finer
12.28
Dissolve the solids in the indicated solvents, add the aqueous solution (A) to the hydrocarbon solution (B) with stirring, and then disperse the antimony oxide in the emulsion.
Fire-Retardant, Water-Repellent, Rot-Proof Canvas Coating
Ingredients
Per Cent
Modified phenol-formaldehyde resin
4
Aroclor 1254
16
Aroclor 5460
4
Antimony Oxide
8
Tricresyl Phosphate
1.5
Aluminum Stearate
0.5
Copper Naphthenate (8% copper)
8
Mica, ground
3
Limestone, ground
6
Iron Oxide, yellow
7
Chrome Orange
2
V M & P Naphtha
40
DSW 379681
STLCOPCB4100453
Properties Of The Aroclor Plasticizers Mobile Liquids Viscous Liquids Soft Resins Brittle Resins
t '/
Solubility
Numerous applications for the Aroclor plasticizers have been suggested and described in the preceding sections of this bulletin. Their success depends on the general inertness of the compounds and on the range and gradation of their physical properties, including physical state, density, viscosity, melting and boiling points, volatility, and solubility. These and other properties, as well as handling and shipping informa tion, are presented in detail in the remainder of the bulletin.
The Aroclor liquids and resins are readily soluble in most common organic solvents and drying oils. Although all Aroclor plasticizers are insoluble in water, the hard, crystalline materials are generally less soluble than the liquids and softer resins. Solubilities of some Aroclor plasticizers are shown in Table 13.
SW 379682
39
STLCOPCB4100454
i
v.
ft
SOLUBILITIES OF AROCLOR PLASTICIZERS IN VARIOUS SOLVENTS
i cS <55 ^
'N
!N
IICO
CO
CO co
co
CO CO
I I GO I
p
I co
III
I CO
co
I CO I CO I CO I CO
CO CO 'co
'co I CO
CO I CO I CO
CO I co
CO CO I CO I co ICO
>I CO
CO CO I CO I CO I CO
CO I CO I CO
CO I co
CO ICO I CO I CO I CO
CO I CO I CO
I <*3I CO CO
I CO I CO
CO I co
CO I CO CO I CO |CO
Ip
I CO
3
I CO
CO
Ip
CO CO
p
CM I CO
CO
I CO
CO I CO I CO
03
>*
03
C5 ~a
"o < o
*0
<t
CJ
o
CO
E
a: o CO
03
"D
00CO
03
c 03
o
CD
,E 1= E<
< <<o
CQ
<c
a>
sz
cCO 03
03 CO
a) o 03
oo
co
cr -
a;
CO
03
!<
sco sCO
03 CJ
!S
<<
o CoO
03
CCOO
Q0J} CL. 0co0
I E
< ICQ :
o
40 DSW 379683
STLC0PCB4100455
1111111
1111
CO CNl OO 1 1 1 1 1 *4* 1 r-
O 1 1 1 1 1 1 co
CM
CO CO 1
1111
CO CO
CO CO 1 -- 1 CO CO
co
vs
VS VS VS VS VS SS
vs vs vs vs
VS VS VS VS VS VS VS VS
vs vs
co CO
CO CO
CO
CO
CO CO
<=> LT3 CO
CO -- CO CO
1 CO 1
1 CO
CO CO 1 1
CO 1 CO co 1 CO CO CO CO
CO -- - 1 CO --
ss
SS SS
ss ss
ss
ss ss ss ss ss
ss
vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs
VS vs VS
vs vs vs vs vs VS
vs vs vs vs
vs vs vs
1 --I
1 CO
---- 1 1
CO 1
co 1 CO CO CO CO
------ 1
--
CO CO CO CO CO CO CO
ooCO
03 03
CO
in
CM
1 oo
C3 r~
CO CO CO CO 00 CO CO
GO J
CO
<N co
CO
r.
CD 1 oC3
CO
CO >
CO
CO
1 CO
o o in CO CO CO CO -- CM CO CO 04 CM
CM
cj gj
CO
CO
CO
O
--
CM LC3
CO
Diethyl Phthalate Ethyl Acetate Ethyl Lactate Methyl Acetate Tricresyl Phosphate her: Ethyl Ether her Alcohol Carbitol' vs Cellosolve Diethylene Glycol
ss
SA
SA SA SS SA
CO CO CO CO CO CO CO
CO 1
CO CO CO CO CO CO CO
CO
1
CO CO
CO CO CO CO CO CO CO
u
03
03 r**-
CO
o
co
C3
03
1
03 03
CO CO CO CO CO CO CO
oc_>
*3 CO
CM CM
03 (0 03 u
503
o o 2>. 13 03 e 03
-= UJ
LU LU
CD
CO
1
CM 03
CO
h. 03 UJ
4-^ UJ
X o o > JCZ CD
V
< zc
vs vs
vs
CO :>
CO
C_3
CO
CO CM
Z> o
CM
CO CO
gj LTD
CO CD CNJ
ydrocarbon Benzene Gasoline Kerosene Mineral Spirits Paraffin Pine iOl Toluene Turpentine Xylene ydroxy derivatives Amyl Alcohol //-Butyl Alcohol Ethyl Alcohol (3-A) Glycerine Methyl Alcohol Phenol -- 90% etone: Acetone
1 1 1- 1 1 1
111
111
ogj 0
oo
CO
CO
C3
--
CO in
CO
CO
C3 OO
CO oo
cj GJ GJ
CO
CO
03 CM CO
-
03 CM in
oCO
CO
CO CM 03
CM
oP
CO IT3
ErTM
03 CO
CJ
DC
I
DSW 379684
Trademarkof UnionCarbideCorp.
41
STLC0PCB4100456
TABLE 14 CHEMICAL AND PHYSICAL PROPERTIES OF REPRESENTATIVE AROCLOR PLASTICIZERS AND RESINS
Property Appearance
Aroclor 1221
Clear, mobile oil
Aroclor 1232
Clear, mobile oil
Aroclor 1242
Clear, mobile oil
Aroclor 1248
Clear, mobile oil
Aroclor 1254
Light-yellow viscous liquid
Color, maximum
*100 APHA
*100 APHA
*100 APHA
*100 APHA
*100 APHA
Chlorine, percent
20.5-21.5
Acidity, mg KOH/g, maximum
`0.014
Moisture, ppm, maximum
--
Are. Coefficient of Expansion, cc/cc/C 0.00071 (15-40C)
Specific Gravity
*1.182-1.192 (25715.5`C)
Density, pounds per gallon, 25C
9.85
Distillation Range, C, corrected (ASTM D-20, modified)
275-320
Evaporation Loss, %, 100C, 6 hours (ASTM D-6, mod.) 163*C, 5 hours
1.0-1.5
Flash Point (Cleveland Open Cup), C 141-150 F 286-302
Fire Point (Cleveland Open Cup), C 176 F 349
Pour Point (ASTM E-97),
C 1 (crystals) F 34 (crystals)
Softening Point (ASTM E-28),
C -- F
Refractive Index, n D-20
20C 1.617-1.618
Viscosity, Seconds Saybolt Universal
(ASTM D-88)
100F (37.8C)
130F (54.4C)
210F (98.9C)
*38-41 35-37 30-31
31.5-32.5
*0.014
--
0.00073 (25-100C)
`1.270-1.280 (25715.5C)
10.55
290-325
1.0-1.5
152-154 305-310
238 460
-35.5 -32
--
1.620-1.622
*44-51 39-41 31-32
42
*0.015
*50
0.00068 (25-65C)
*1.381-1.392 (25715.5C)
11.50
325-366
0-0.4 3.0-3.6
176-180 348-356
None to boiling point
-19 2
--
1.627-1.629
*82-92 49-56 34-35
48
*0.010
*50
0.00070 (25-65C)
`1.405-1.415 (65715.5C)
12.04
340-375
0-0.3 3.0-4.0
193-196 379-384
None to boiling point
-7 19.4
--
1.630-1.631
185-240 *73-80 36-37
54
*0.010
*50
0.00066 (25*-65C)
*1.495-1.505 (65715.5"C)
12.82
365-390
0-0.2 1.1-1.3
None to boiling point
None to boiling point
10 50
--
1.639-1.641
1800-2500 260-340 *44-48
'Monsanto Spocfftcatkms
DSW 379685
STLCOPCB4100457
Aroclor 1260
Light-yellow, soft. sticky resin
*150 APHA
60
*0.014
*50
0.00067 (20-1007)
*1.555-1.566 (90715.57)
13.50
385-420
0-0.1 0.5-0.8
None to boiling point
None to boiling point
31 88
1.647-1.649
Aroclor 1262
Aroclor 5442
Light-yellow sticky, viscous resin
Clear yellow sticky resin
*150 APHA
*2 NPA (molten)
61.5-62.5 *0.014
42 *0.05
----
0.00064 (25-65C)
0.00123 (25-99C)
*1.572-1.583 (90715.57)
1.470 (257257)
13.72 12.24
390-425
215-300 (4 mm. Hg)
0-0.1 0.5-0.6
0.01 0.2
None to boiling point
247 477
None to boiling point
>350 >662
35-38 99
46 115
*46-52 115-126
1.6501-1.6517 --
Aroclor 4465
Clear, light-yellow. resin
*2 NPA (molten)
65
*0.05
--
0.00061 (25-65C)
1.670 (257257)
13.91
230-320 (4 mm. Hg)
0-0.02 0.2-0.3
None to boiling point
None to boiling point
_
*60-66 140-151
1.664-1.667
Aroclor 2565
Aroclor 5460
Aroclor 1268
Black, opaque. brittle resin
Clear, yellowto-amber. brittle resin or flakes
White to off-white powder
*2 NPA (molten)
*1.5 NPA (molten)
65
58.5-60.6
68
*1.4 *0.05 *0.05
---- --
0.00066 (25-657)
0.00179 (25-1247)
0.00067 (20M007)
1.734 (257257)
1.670 (257257)
1.804-1.811 (257257)
14.44 13.91 15.09
280-335 (5 mm. Hg)
435-450
0.2-0.3
0.03
0-0.06 0.1-0.2
None to boiling point
None to boiling point
None to boiling point
_
None to boiling point
_
*66-72 149-162
--
*98-105 208-222
1.660-1.665
*150-170 (hold 302-338 point)
--
3200-4500 *72-78
600-850
(1607; 71C) *86-100
300-400
90-150
--
(2667; 1307)
--
--
DSW 379686
43
STLC0PCB4100458
Density
All the Aroclor plasticizers are heavier than water, a valuable property for many applications. Densities are shown in Figure 2.
Specific Volume
Fig. 2 -- Densities of Aroclor Plasticizers at Various Temperatures
The specific volume of Aroclor 1248 at different temperatures is as follows:
Temperature (F) 0 100 200 300 400
Aroclor 1248 Specific Volume (mijg)
0.674 0.699 0.726 0.755 0.790
500 0.828
600 0.870
DSW 379687
STLCOPCB4100459
Volatility
The low vaporization loss of Aroclor plasticizers is indicated in Table 15.
TABLE 15
VAPORIZATION RATES OF AROCLOR PLASTICIZERS
Plasticizer (Surface area: 12.28 sq. cm.) Aroclor 1221 Aroclor 1232 Aroclor 1242 Aroclor 1248 Ciorafin'-42-S Dioctyl phthalate Outrex" 25 Aroclor 1254 Shell Dutrex 20 Aroclor 1262 Aroclor 1260
Wt. Loss (9)
0.5125 0.2572 0.0995 0.0448 0.0745 0.0686 0.0256 0.0156 0.0047 0.0039 0.0026
Exposure at 100C
(hr.) 24 24 24 24 48 48 24 24 24 24 24
Vaporization Rate
(glsq. cm./hr.) 0.00174 0.000874 0.000338 0.000152 0.000126 0.000117 0.000087 0.000053 0.000016 0.000013 0.000009
Aroclor 4465 Aroclor 5442
0.0064 0.0039
72 72
0.000007 0.000004
Aroclor 5460
0.0032
72
0.000004
Tricresyl phosphate
0.0010
24
0.000003
It is concluded that the vaporization rates of Aroclor plasticizers -- especially the most widely used 1254 and 1260 -- compare most favorably with the similar constants of other plasticizers selected specifically for these tests because of their low vaporization rates.
'Trademark of H*rcui*,1i>c. ~T4Ni*rk of Sfwll Oil Co.
DSW 379688
45
STLCOPCB4100460
Vapor Pressure
The vapor pressures of several Aroclor plasticizers are indicated in Figure 3 over the temperature range 150 to 300C.
!
i
9
1
i
i i i
Temperature, C
Fig. 3 -- Vapor Pressures of Aroclor Plasticizers
The estimated vapor pressures of several Aroclor plasticizers at 100F shown in the following table were determined by extrapolation from the values shown in Figure 3.
Approximate Vapor Pressure of Aroclor Plasticizers Estimated at 100 F (37.8 C)
Aroclor 1232
0.005 mm. Hg
Aroclor 1242
0.001 mm. Hg
Aroclor 1248
0.00037 mm. Hg
Aroclor 1254
0.00006 mm. Hg
DSW 379689
46
STLCOPCB4100461
Viscosity
The viscosities of the Aroclor plasticizers vary according to whether the base material is a biphenyl or a polyphenyl and on the degree of chlorination. In general the low-chlorinated biphenyls have the lowest viscosities (Figure 4).
Stability
Toward Alkalies The Aroclor plasticizers are remarkably resistant to the action of either hydrolyzing agents or high temperature. They are not affected by boiling with sodium hydroxide solution.
Toward Acids No hydrogen chloride was evolved when Aroclor 1254 was stirred with an equal volume of 10 percent sulfuric acid for 150 hours. Even after prolonged treatment (255 hours) with concentrated sulfuric acid only a slight trace (too small for quantitative measurement) of hydrogen chloride was evolved.
Toward Heat Because of their stability to heat, the Aroclor plasticizers are useful heat-transfer media. Aroclor 1254 and particularly the less viscous Aroclor 1248 are recommended for this purpose, because they may be heated up to 315C (600F) in a closed system for long periods without appreciable decomposition, and because they are nonflammable.
Toward Light The Aroclor plasticizers have good light stability in heavily pigmented compounds and fair light stability in clear formulations. The materials become discolored, but their physical properties are not degraded. For critical applications, incorporation of a small amount of a light-
DSW 379690
47
STLCOPCB4100462
screening agent greatly improves light stability at reasonable cost. The following data show that as little as 0.01 percent Tinuvin P in Aroelor 1254 nearly doubles the service life in the 50-to-100-hour range and that 0.1 percent Tinuvin P results in a 10-fold improvement.
Tinuvin P Concentration (%J
Fade-Ometer Exposure (hours)
0 SO 100 150 500 Color (Gardner Units)
0 0 5 10 11 14
0.01 0 1 6 7 14
0.05 0 0 3 4 11
0.1 0 0 1 2 6
Toward Oxidation
When Aroelor plasticizers are heated to 140C with oxygen in a bomb at 250 psi, no evidence of oxidation occurs, as judged by absence of sludge formation or increased acidity. Also, no increase in acidity occurred after 4 hours heating with air at 260C and 210 psi.
Nonflammability
The viscous Aroelor liquids and the resins do not support combustion when heated alone, even at their boiling points -- above 350C. Most of the Aroelor plasticizers flux readily with resinous and pitch-like materials to give products with decreased fire hazard. Aroelor products incorporated in plastic products and rubber foams retard the rate of burning.
Nondrying Properties And Thermoplasticity
The Aroelor plasticizers are nondrying. When exposed to the air, even in thin films, no noticable oxidation or hardening takes place. Despite this property, Aroelor plasticizers do not retard the drying rate of lacquer films. Quick-drying varnishes and paints may be made with Aroelor resins without affect on drying characteristics.
The Aroelor plasticizers are permanently thermoplastic. They appar ently undergo no condensation or hardening upon repeated melting and cooling. Clear Aroelor resins are available with softening points up to 105C. The opaque crystalline solids are available with melting points up to about 160C.
El metrical Properties
The electrical properties of Aroelor plasticizers are extremely interest ing: high resistivity and dielectric strength and low power factor, as listed in Table 16. The dielectric constants of the various Aroelor plasticizers range from 3.3 to 4.9 at 100C and 1000 cycles.
48
1
1 I
STLCOPCB4100463
How To Emulsify Aroclor
TABLE 16
ELECTRICAL PROPERTIES OF AROCLOR
Volume
Dielectric
Resistivity
Power
Constant
(ASTM D-257-46) Dielectric
Factor
(ASTM D-150-47T) 500 Volts D.C.,
Strength (ASTM D-150-47T)
1000 cycles
100C
(ASTM D-149-44) 1000 cycles. 100C
Aroclor 25C 100C
(ohm-cm.)
(KV)
(%)
1232 5.7 4.6
1242 5.8 4.9 Above 500 x 109 Above 35
Below 0.1
1248 5.6 4.6 Above 500 x 109 Above 35
Below 0.1
1254 5.0 4.3 Above 500 x 109 Above 35
Below 0.1
1260 4.3 3.7 Above 500 x 109 Above 35
Below 0.1
1268 2.5
5442 3.0 4.9 Above 500 x 109 5454 2.7 4.2 5460 2.5 3.7
4465 2.7 3.3
Emulsions of Aroclor plasticizers can be made simply in several ways; the method can be selected to suit the particular Aroclor and the type of formulation in which it will be used.
Emulsifiable Concentrated Stock Solutions of Aroclor
Stock solutions made according to the following formulation are readily emulsified with water. The amount of toluene may be increased as needed to dissolve the more resinous Aroclor plasticizers.
Ingredient Aroclor Toluene Isopropanol Sterox CD (nonionic emulsifier) Santomerse No. 3 (anionic wetting agent)
Parts by Weight 79 16.70 3.55 1.00 0.75
Emulsifying Liquid Aroclor Ingredient Portion 1 Aroclor 1254 Oleic Acid
Portion 2 Water Ammonium Hydroxide (28%)
Parts by Weight
100 4
100 2
DSW 379692
49
STLCOPCB4100464
Mix the polystyrene and ammonium hydroxide in warmed water with vigorous agitation. Mix the Aroclor 1254 and oleic acid, heat to 45C, and agitate vigorously. Maintain the 45C temperature and agitation, and slowly add in the aqueous portion (Portion 2). Continue agitation for one-half hour until phase inversion is complete.
Emulsifying Viscous Aroclor Ingredient Portion 1 Aroclor 1254 Stearic Acid
Portion 2 Water Triethanolamine
Parts by Weight
64 4
32 1
Heat the Aroclor to a workable viscosity (180F or higher) and stir in the stearic acid thoroughly. Heat the water almost to boiling (207F) and stir in the triethanolamine thoroughly. Pour the Aroclor-stearic acid portion into the water-triethanolamine portion with vigorous agitation. Process the combined portions either with a high-speed emulsifying stirrer or through a colloid mill.
Toxicity And Safe Handling
Inhalation
At ordinary temperatures the Aroclor chlorinated polyphenyls have not presented industrial toxicological problems. The hazard of potential toxic exposure varies with their volatility: the lower-chlorinated, morevolatile ones present more of a potential problem from the standpoint of both inhalation and skin contact. When Aroclor plasticizers are used at elevated temperatures, engineering controls must be applied, either by the use of closed systems or by effective local-exhaust ventilation together with general workroom exhaust.
Vapor of the liquid Aroclor plasticizers at room temperature should not be breathed in a confined space, and no vapor of any Aroclor evolved at elevated temperatures should be allowed to be dispersed into the general workroom.
Inhalation tests on animals indicate that the maximum safe concen tration of vapor is in the range of from 0.5 to 1.0 milligram of the lower-chlorinated Aroclor plasticizers per cubic meter of air. The threshold limits (maximum allowable concentration for an 8-hour working day) set by the American Conference of Government Hygien ists are 1.0 milligram of the lower-chlorinated Aroclor compounds per cubic meter of air and 0.5 milligram of the more-highly-chlorinated compounds, such as Aroclor 1254, per cubic meter of air.
Skin Contact
Schwartz patch tests on 200 volunteers showed that Aroclor 1254 was neither a primary skin irritant or a sensitizer.
DSW 379693
;
I
r l
STLCOPCB4100465
Shipping
Continuous or repeated skin contact with the Aroclor plasticizers must be avoided by the use of gloves and protective garments, because of the possible occurrence of a condition called chloracne. Although reports of this condition caused by Aroclor are rare, it can be produced by excessive skin contact. If any Aroclor is spilled on the skin the skin should be washed in the usual manner with a soap solution.
A bum caused by contact with a hot Aroclor should be treated like any ordinary bum. Aroclor plasticizer adhering to the burned area need not be removed immediately, unless treatment of the bum demands it, in which case either soap and water or repeated washings with a vegetable oil are recommended.
Freight Classification
Aroclor 1221, 1243, 1242, 1248, 1254, 1260, 1262
Synthetic Resin, Liquid, NOIBN
Rail Classification
Aroclor 1268, 2565, 4465, 5442, 5460
Synthetic Resin, Other Than Liquid, NOIBN
Truck Classification Aroclor 1268, 2565 Aroclor 4465, 5442, 5460
Synthetic Resin, Powder, NOI
Synthetic Resin, Lumps or Solid Mass, NOI
Shipping Regulations
None
Standard Containers Aroclor 1221
Aroclor 1232
Aroclor 1242, 1248, 1254, 1260, 1262
Aroclor 1268
Aroclor 2565, 4465 Aroclor 5442 Aroclor 5460 (flaked)
Tank car, 520-lb. steel drum, 50-lb. can
Tank car, 550-lb. steel drum, 50-lb. can
Tank car, 600-lb. steel drum, 50-lb. can
200-lb. fiber drum, 25-lb. fiber drum
500-lb. steel drum, 50-lb. can
450-lb. steel drum, 50-lb. can
100-lb. bag
dS\N 379694
51
STLCOPCB4100466
DISTRICT SALES OFFICES ALL DIVISIONS
ATLANTA, GEORGIA 30326
Lenox Towers East 3400 Peechtree Pd. N. F. -- Suite 1711 Tel. (404) 577-2260
BOSTON, MASSACHUSETTS 02149
Everett Stetion Tel. (617) 387-5010
CHICAGO, ILLINOIS
3158 Des Plaines Ave. Des Plaines, Illinois 60018 Tel. (312) 296-6688
CINCINNATI, OHIO 45206
1501 Madison Road Tel. (513) 751-6707
CLEVELAND, OHIO 44122
3645 Warrensville Center Rd. Tel. (216) 991-5400
DETROIT, MICHIGAN 48235
500 Northland Towers East
Tel. (313) 357-0910
HONOLULU, HAWAII 96812
205 Pacific International Bldg. 677 Ala Moana Blvd., P. 0. Box 3824
Tel. (808) 512-744
HOUSTON, TEXAS 77002
1300 Main Street Tel. (713) Capitol 3-4011
LOS ANGELES, CALIFORNIA 90022
6670 . Flotilla SL Tel. (213) 723-2492
MINNEAPOLIS, MINNESOTA 55402
912 Northstar Center 110 S. Seventh SL
Tel. (612) 339-4651
NEW YORK, NEW YORK 10017
277 Park Avenue Tel. (212) 922-4111
PITTSBURGH, PENNSYLVANIA 15222
No. 4 Gateway Center Bldg. Room 534 Tel. (412) 261-2156
ST. LOUIS. MISSOURI 63166
800 N. Lindbergh Blvd. Tel. (314) Oxford 4-1000
SAN FRANCISCO BAY AREA
2710 Lafayette, Santa Clara. Calif. 95052
Tel. (408) 243-0414
SEATTLE. WASHINGTON 98104
911 Western Avenue Tel. (206) Main 2-4203
SPRINGFIELD, MASSACHUSETTS 01101
730 Worcester Ave. Tel. (413) 788-6911
WILMINGTON. DELAWARE 19803
2005 Concord Pike. Fairfax
Tel. (302) Olympia 8-6531
-
Additional District Offices are maintained by:
Agricultural Division
LULING. LOUISIANA 70070 P. 0. Box 174 Tel. (504) 784-6283
MEMPHIS. TENNESSEE 38113 1023 Riverside Orive P.O. Box 13248 Tel. (901) Whitehall 7-3151
Textiles Division
AKRON. OHIO 44313 3030 West Market St Tel. (216) 836-7941
ATLANTA. GEORGIA 30303 Atlanta Merchandise Mart 240 Peachtree St. N. W. Tel. (404) 577-2260
CHARLOTTE, NORTH CAROLINA 28202 Wachovia Bank Building 129 West Trade St Tel. (704) 376-9871
ENGLEWOOD CLIFFS. N. J. 07631 661 Palisades Ave. Tel. (201) 568-2151
NEW YORK. NEW YORK 350 Fifth Ave. Tel. (201) 556-5100
Hydrocarbons & Polymers Division-Lion Oil
EL DORADO. ARKANSAS 71730 Uon Oil Building Tel. (601) Union 3-3111
JACKSON. MISSISSIPPI 39209 P. O. Box 10937 Westland Station Tel. (601) 352-3648
LITTLE ROCK. ARKANSAS 72203 1515 West Seventh St Tel. (501) Franklin 0-2437
MEMPHIS. TENNESSEE 38113 1023 Riverside Drive P. O. Box 13248 Tel. (901) Whitehall 7-3151
Organic Chemicals Division (Rubber Industry)
AKRON. OHIO 44311 920 Brown Street P. O. Box 2307 TeL (216) Hemlock 4-1921
MONSANTO. 800 N. LINDBERGH BLVD.. ST. LOUIS, MISSOURI 63166
J
1-2-68
DSW 379695
2-2713-0568-6 LITHO IN U.S.A.
STLCOPCB4100467
DSW 379696
MQNSANJQ, 800 N. LINDBERGH BLVD.. ST. LOUIS, MISSOURI 63166
STLC0PCB4100468