Document yk7knEnOB6q51ao3JqdBQm8OE
V esisufti# ELECTSI.G
.' Telephone: 38.9-7011
C* . . ' "7
DIAL COMM: 8*272-7 .
INDUSTRY CONTROL DEPARTMENT, 1501 Roanoke Boulevard, Salem,.Virginia 24153
. * ,, .baybestos-manhattm BRAKE LIMING
. ";
.
GR. Ktumiiacher - Room D431 FL Breariey - Room D431 DM Morley - Room- 101L JM Burnley -- Room 166
August 13, 1969 Salem, Virginia
.^ . t'
"Mr. AvEi. Coulter Room 141
Please be advised that this. letter cons titutes,. engineering- approval of the, R-M #G15Q0 woven brake lining for use on all part, numbers of our drawing 151A4453. The print will be changed accordingly in the next"few days.
Concerning the evaluation samples of R-M banded brake linings, t am listing the test values for record purposes, I suggest you send a copy to RaybestosManhat.tan so they will'be aiware of what improvements .they have to make-before final, approval for production dan be given. * -
XC9528 "A" brake bonded lining (151A7931P3)' .
** *
Ro Sample
13,000# Proof Load
/In. lbs) Rupture
Point
Reason for, ..Failure
... , ' -
'
:
1 2 3 4' 5 A
7
a.
** . l - 117-:'
v ; v ; 11 .
.: -
iz
\ . 13;
14
^
1*
-OR . OK. OK 'OK
OK ntr
OK
OK OK . QK ", -'OK
... . *K - -OK ; K' -
`
23,750 34,700 40,000 38,200 41,500. W, son
33,500 48,000 44,500 50;200
50,100 . 41,500: 36,000
4d;100 31,500
Mat* crushed Mat'd crushed . . Mat11 crushed Bond Failed Ma&'L crushed. Bund Fa-51 p.d
.Mat*1 crashed Mat'.l crushed Bond Failed Bond Railed .Bond Failed' Mat'l crushed Mat'l crushed Mat*i crushed Mat',l crushed
. 16 .
\
*-17
T :is .
. 19
ELEVATED TEMPERATURE FOR 48 HOURS
150F OK 250V OK 350F OK 400F OK
32,200 13,700 20,000 21,000
.
Bond.Failed Bond Failed Bond Failed Bond- Failed
'3!'Bond Coverage
75-80% 0-70% ..
-. . 85-40%. . 90%
95% . 95%
*" T . I '.'V- .........
50-60% 40-50% *
X
*
.v
J
.
'
|4 .. ...
;
'\ *
PLAINTIFF'S EXHIBIT
WV'02!53t
PLAINTIFF'S EXHIBIT
GEWVOCT04-011705
. Page Two Mr. A. E, Coulter
- ' August 13, 1969
No, Sample
13,000# Proof. Load..
(In lbs)
Rupture Point
Reason for ' Failure
AT 100% HUMIDITY FOR 48 HOURS
___________:__________:L__________________ r___________^*
2Q .21
12 23:
OK '
ok
.. $K :'m
'
33,000
Mat*!" crushed
- *?t0O0 . ' . . Bond Failed . 32*000 ; Mat*! crushed
; 25,000 ; L Mat'd crushed . t,
, s...k\.'; i.... --, V:. .
'
;.
IC9528 "C'* Brake bonded lining (167A8474P3)'
... No, Sample 13,00.0# Proof .Load .. .
t . j-
'V .
2 3 4
OK ` ! . m
m.i : : ok
o m$-' ..".`Reason for-
Rupture
Failure
Point'-
.......;
''
46,800: J Bond.Failed
42,600
Bon#: Failed
42*500 : j ,, Mat'5!'crushed
M,mo - .j y Mat'1-crushed
%. Bond Coverage
w* *.
6o% . '
~
X Bond Coverage
98% 95%.
t.
t' .
ygVAiEB TEMPEBAsEPRE'
48 HOURS' ' .
'
5 ; 6.
* %
ok OK
30;OOO . 31,000
; .. Bond Failed . ?:V Bond: Failed
...
. -.
7',:.
OK ..
.avsffl?...
----&----- --i-- X--gs
:-------------------
TM nnh .
' 9'
OK
34,000 y
. f' MatwX crushed ... Mat! 3 ei-iished
Mat!!' crushed
' ' m : . 80% / `
' .v r-
_
' . *-
Please, point out .to Mr-. 'Carl Walker that the bond coverage bn some samples were on .the sklaipy^slde. In fact, sample number .17 ^ubt barely madetheproofload test. This Indicates need' for soma definite action on their .pat't in their
bonding, process /Other than this point* -the material and bond strength .is .almost ' 100% higher thdn. the ones furnished by iqhns-Manville. We catmot Start any
rotational tests, such as.fade, wear rate, life, etc. until we receive four bonded I-ihitig assemblies1 which are dimensionally per-drawing, as the sheets angles were . .
tf:. Mt. Waljcer agreed to'push this procurement for us.
0op(lknd
IpDUCT, PRODUCTION & DEVICE. ENGINEERING am D431 *- Ext,' 604
GEWVOCT04-011706