SALESMEN'3 MANUAL AROCLOR
DESCRIPTION AND PROPERTIES
The Aroolors are a series of chlorinated hydrocarbons based on biphenyl and terphenyl. They are not pure compounds but are
mixtures of olosely Telated chlorine substitution products man ufactured essentially to a set of specifications based on physical properties rather than chemical composition.
The approximate chlorine content is indicated by the last two figures of the Aroclor number. The chemical composition closely approaches the average for the indicated chloro-derlvatlves as follows,but should not be represented as simple chemical compo sitions according to the formula shown:
Approximate Equivalent Chemical Compound
1239+1 1232 1242
1248
1254
1260 1262 1268
1271 5460
Monochloroblphenyl Dlchloroblphenyl Trlchloroblphenyl Tetrachlcroblphenyl Pentachloroblphenyl Hexachloroblphenyl Heptachloroblphenyl Nonachloroblphenyl Decachloroblphenyl Nonachloroterphenyl
Reference should be made to technical bulletin P-115 for tables and graphs of physical properties. This manual contains only that information which is not designed for general public distribution or has been made more recently available than permitted incorpora tion in the printed bulletin.
The following Aroolors not in commercial production (but available) have been proposed:
Aroclor No.
5448
5454
Fixed Chlorine Polor (I.ovlbond) Pour Point Softening Point
47.9# 6.0
60C 63C
54.83# 20.0 84C 85C
09^643 mqns
MONSANTO CHEMICAL COMPANY
10-1-44
Aroclor No.
5448
Viscosity 98.9OC (210P) 395-0*
-
Flash Point Burn Point
250 C
-
400C
Chlorides Acidity - mg. KOH/g.
Evaporation
None 0.008
0.006
None 0.004
0.007
Resistivity Ageing Dlelectrlo Constant
SOS
4.65
ELECTRICAL PH0PERTIE3
4-iO
4 ^ / > Aroclor Aroolor Aroclor Aroolor
, ^ y 1248
1254
1260
5442
Dleleotrla Constant 9 li>0d
4.63 4.15-4.35 3 -6-3.8 4.92
Resistivity 9 100C, 0HMS/Cm3 AC.
Dielectric Strength
500x 10? > b o v e ,, Above iOOxlO? 500x10?
3^"k V Min.
1469x10?
Power Factor (100C 1000 ko) Less than
0.1#
Less than O.ljS
IRS Method H-3955871 Resistivity 9 100 under 500 Volts DC
ASTM D.177-11
Refractive Index
Range
Midpoint
Aroclor 1270 Aroclor 1271 Tetradecaohlorometaterphenyl Tetradecaohloroparatorphenyl
1.691-1.74 1.691-1.74 1.712-1.718 1.691-1.74
Heat of Vaporisation
Aroolor 1260 (3 mm. pressure)
Aroolor 1262 (760 mm. pressure) Aroclor 1169 (O.151 atm. 9 350C)
(0.079 atm. 9 325C)
1.712 1.712
-1.712
B.I.U./lb.
104 72.4 69.2 70.6
-2-
MOhS 091644
MONSANTO CHEMICAL COMPANY
10-1 -44
SOLUBILITY
Solvent
Acetone Alcohol, Formula J-A Amyl Acetate Amyl Alcohol Benzene Butyl Acetate N. Butyl Alcohol Carbltol
Chloroform D1 Butyl Phthalate Ether Ethyl Acetate Ethyl Lactate Ethylene Bichloride
40% Formaldehyde
Furfural High Test Gasoline Glycerin Kerosene Linseed Oil Methyl Acetate Mineral Spirits Paraffin Phenol 90% Pine Oil Pyridine Toluene Trl Cresyl Phosphate Tung Oil Turpentine Xylene
Aroclor 1268
Cold
Hot
X
I
X
I
s
S
PS
8
8
8
S
S
I
PS
I
s
7
s
S
3
3
S
S
PS
PS
I
s
s
s
I
I
PS
PS
I
I
PS
s
I
s
PS
PS
S*r
PS s s s s
tr
3 s s s s
J* ^e-ro'c.
JVC
I . Insoluble PS Partially Soluble
S Soluble
Solvent
Gas. Aroolor 1270
per 100 cc.Solvent
Approx. Temp, at vhlch soln.oomplete
Furfural
2.0
Furfural
4.0
Secondary Amyl Acetate
4.0
Secondary Amyl Alcohols
4.0
Carbltol
4.0
Heavy White Mineral Oil
4.0
105-110OC 120-125C
1 1 0 .1150c
Not completely soluble at boll
Above 125C 110-115C
MOMS 092O'*5
MONSANTO CHEMICAL COMPANY STABILITY
10*1-4*
Toward Heat
Aroclor 1248 was heated to 650P In stainless steel autoclave with the resulting changes indicated In the following tabulation:
Original Sample Autoclave #1 Autoclave #2 Autoclavo #3
Time of Heating (Hours)
0
331
500 669
Temper ature
__
343C. 6500?. 343C. 650?.
3430C. 650?.
Acidity mg.NaOH/gm. Aroclor 1248
.0021
.0392 .0809
.0800
Those results are interpreted as indicating very.excellent stabil ity for Aroclors under the conditions of test.
Toward Oxidation
When Aroclor 1254 is heated for 50 or 60 days at 150C in the presence of oxygen and copper, there is likely to be some attack on the copper. Examination of Aroclor 125* after that period of time will usually show the presence of soluble copper. This also occurs with mineral oil and other lnsulat ng liquids.
In general, even after severe oxidation conditions no evidence of chlorine splitting from the parent hydrocarbon has. been found.
Toward Acids ,
Aroclors 1242 and 125* were stirred with an equal volume- of con centrated Suirurlc Acid (96jS), dilute Sulfuric Acid (10J(), Nitric Acid (70%), and dilute Nitric Acid (5%), at room temperature (25C) for 150-250 hours. The Aroclor was then washed until neutral, de hydrated with Sodium Sulfate, then analyzed in comparison with a control sample for the various properties Which are regularly con sidered, without causing these properties to depart from specifica tion limits.
Aroclor 1262 was treated for 160 hours suspended in the same acids
as above at 50 to 55C. The concentrated Nitric Acid caused an inorease in color, otherwise no significant change in characteris tics.
The acid layer from the treatment of Aroclor 1254 was concentrated Sulfuric Acid at room temperature for 150 hours and vas tested for chloride content. The quantity of HC1 found was so small that it was not possible by ordinary methods to obtain a quantitative fig ure. Thus it appears that practically no hydrogen chloride is evolved under these conditions.
-4--
q 9 26M>
mons
SSL-
MONSANTO CHEMICAL COMPANY COKROSIOil
10-1-44
Additional cirrosion data hot included in bulletin P-115 (PI 4-43-R)
la aa follows:
t
Metal
Tamperature
. Tiara of Exposure
Penetration ln/yr.
Monel Doe Metal Telloe Braea
342C 150C 325C
A1 alloy 17ST 120OC
A1 alloy 528H 120C A1 alloy 53ST 120C
360 hra. 40 daya
2,960 hra.
in ateel bomb
21 21
21
.008
.001
,003
.00035* .00035* .00038*
The weight loaa occurred in the flrat seven daya of the test, negligible loss vas encountered in the last 14 daya.
The vapor condenser and the product receiver of the plant distilla tion unit for producing Aroclor 1254 la constructed of Monel and no failure in the system nor any noticeable reaction betveen the Aroolor and the Monel has been discovered after three years of opera tion.
SOLUBILITY OF WATER IN AROCLOR 1242
The water content of a sample of Aroclor 1242 saturated with water
at approximately 30C was determined,using the Karl Plscher reagent,
to be about 0.080.
......
Aroclor 1242, as regularly produced, contains by the same test less
than 0.0010 water,
SOBPACB TEWSIOH The surface tension of Aroclor 1254 is as follows:
Temperature
25 C
80C
100C
Dynes per Centimeter
50.}
'
44.0
42.0
wxiom
v
All chlorinated hydrocarbons have measurable degrees of toxicity,'t
the animal organism. Ardclors are no exception. The symptoms of
Aroolor poisoning ore: '
-A
..
1. Pore acne (chlor-aehe)nodular eruptions the hair follicles or sebaceous glands as a result of
... insufficient cleansing of the s k i n ' . " ~
- - ^.--4.
** v*- *
.-'ihrL-~i ssieti3SK-'-uvsm
MONSAHTO CHEMICAL COMPANY
10-1-4*
3. Acute yellow atrophy of the liver In wbleh the liver oelle show evening, hypergranulation, hyaline lneluelone and vacuolatlon ae a result of extensive, expo sure over long periods of tlise.
These symptoms may aleo result frosi exposure to other chlorinated hydrocarbons of ooetneroe, such sat carbon tetrachloride, dlchlorethylene, trlohlor ethylene, ohlorlnated naphthalene (Halowex). The best knovn (at present) measure of the degree of toxicity of the Aroolors is presented below
Permissible Limits (in mg./ou.m.) of Concentration In Air of
Work Rooms: (journal or Industrial Hygiene a Toxicology 3 l :
1'55."19J9)
~
Tested on Rats by Inhalation
Chlorine Permissible
Content
Limit
___1 -
Aroolor 1368
68
10.0
Aroclor 4465 Aroolor 5460
6605
0.5 0.5
Aroolor 1354
c
Trlchlornaphthalene plus trace Tetrachlornaphthalene
Tetra and Pentachlornaphthalenes
54 49.9
56.1
0.5
10.0 1.0
Penta and Hexaohlornaphthalenes
63.6
0.5 *
Tetra and Pentaohlornaphthalenes plus
Refined Chlorinated Diphenyl 900 Penta and Hexaohlornaphthalenes / 10J<
4?. 5
0.5 *
Aroolor 4465 Chlorinated Diphenyl Oxide Chlorinated Diphenyl Oxide
63.0 54.0 57.0
0.5 * 0.5
0.5
Bexachlor Diphenyl Oxide / 5j< Trlchlor
naphthalene
50-55
0-5
Rexachlornaphthalene and Crude Chlorinated
Diphenyl
0.5
Special Chlorinated Naphthalene
50-56
0.5
Tested also by feeding."
Summary of Prose Needing Experiments
Of the various materials fed rats in large doses, Trlchlornaphthalene
plus traces of Tetrachlornaphthalene was quite Innocuous. Tetra
and Pentaohlornaphthalene showed definite liver damage. Penta and
Hexaohlornaphthalenes caused a similar grade of Injury. The addi
tion of chlorinated diphenyl to Penta and Hexaohlornaphthalenes
lnoreaeed the toxlelty. Chlorinated Diphenyl alone produced liver
lesions but In the dosage used vae leas effeotlye than when'mixed
l
with highly chlorinated naphthalenes. In no ease" did the compounds
HONS o s j o y a
MORSAllTO CHEMICAL COMPARE
lO-l-^l if
cate this night he possible If one found a dosage vhloh could act for the proper period of time.
Feodlng Precise Poses by Stomach Tube: The compounds employed sere
suspended in gun hcaela. In figuring the dosage this total amount
a nan of 50 kg. vould inhale In an 8-hour day, assuming on air con
centration of 20 ngm. per cu.m., sas first calculated and reduced
to milligrams per kilogram. Tbs rats and rabbits received this
dose each day. Tho compounds ueed sere those employed ili the gross
feeding experiments and the results were essentially similar though
the lesions sere less severe.
- *
Subcutaneous Injections* 'The some gun acacia suspensions were lnjeoted suboufahoously'Into rate end rabbits, the dosage being cal culated on the basis of k ngm. per ou.m. of air. Again similar results sere obtained. In all such experiments there must of nec essity be differences In the degree of effect but invariably the liver sas the sole organ affeoted and the lesions sere those already deserlbed many times.
Recommendations for Industrial Practice: Unless there Is a very
good reason for using the hot method o? Impregnation, all new' In stallations should use the cold or solvent method of impregnation with chlorinated naphthalenee and diphenyls. Where the hot method Is now being usod It should be changed over to cold, If possible, or surrounded with every known protective measure.
General hygienic measures should be followed, but In no ease should these be allowed to supersede engineering control of the primary souroe of the exposure, the operations in the plant.
The following hyglonio measures may be considered good practlee where these compounds are handledi
(a) Two lockers for each worker exposed to chlorinated saxes (one for working and one for street olothes).
(b) All work clothes above the underwear should be pro
vided and laundered .at,, least `twice a veek, by the
management. .
,, ';A
'(o) The workers should change to clean underwear at tha and of each shift before getting into his street olothes.
(d) Supervised cleaning; (l) At noon the workers should remove outer clothing and sorub hands and faoe under supervision] (2) at the end of the shift they should be required to take a supervised shover.before changing back to treat Olothea . ..-*-
MONS 0 92 6*9
KOlttAHTO CHEMICAL COMPANY
10-1-M
(e) Protective skin creams or protective clothing should be provided by the management at the discretion of the fore man, nurse, medloal, or plant superintendent*
(f) All departments handling chlorinated synthetic vaxes should be thoroughly cleaned according to a prearranged sohedule. This should include the removal of all de posits of waxy material from the maohines. floors and surrounding objects. Workers doing the cleaning should be provided with protective clothing and supplied air or organic vapor masks vhere exhaust ventilation is inade quate or not possible.
The foremen of all departments vhere this material is handled should be apprised of the toxic nature of the material and in structed in aafe handling procedures. These men should make it their duty to cheok up on the workers In their departments and Instruct them in safe practice.
Pre-employment and periodic physical examinations should be made
of all expoaed workers. These should include the taking of a full
clinical history, with special emphasis on gaetro-lntestinal dis
turbances and dermatitis. In addition, the skin should be care
fully examined periodically and the more reliable liver function
taste performed. Oastro-lntestinal complaints developing in a
vorker at any time should be a signal .for an immediate medical
oheok-up. A history of liver disease. Jaundice, or antlsyphllltic
treatment should automatically exolude a worker from Jobe involv
ing a possible toxic exposure. Pregnant women should not be em
ployed where there is a possible exposure to the synthetlo chlor
inated waxes,
.
Engineering control of plant operations oannot be over-emphasised but specific recommendations are not applicable to all oases, it would be vise for a plant using this class of materials to check their oontrol measures with the state industrial hygiene agency, the insurance carrier and Some competent consultant before occu pational disease' oooura............
APPLICATIONS OP AR0CL0R3
AbHBSIVBS
Adhesives of good, electrical characteristics oan be prepared con taining Aroolors. The following are typioal examples:
#103 (XV)
Aroelo* *U65 (Code JlkO-OlW) Paraffin 50.600 Mineral Oil (Ext(pa Heavy White) Barytes - Met>ham*s #2
Typical Values
MONSANTO CHEMICAL COMPANY
10-1 -**
(
Typical Values
#103B Aroclor 2565 (S.P. 77.5C) (Code 31*0-011*) (XB) Paraffin 50.8C
Mineral Oil (Extra Heavy White - Sonneborn 'e) Barytes - Mepham's #2
*6.50#
1.17 8.33 50.00
#131 B-ll
65B
Aroclor **65 (Code 31*0-01**) Ester Oum - BKEO #1202XXXX Pale Paraffin 50.8C Barytes - Nephan's #2
16 .10#
15.35 *.55
. 65.00
#135
Aroclor **65 (Cods 31*0-01**) Ester OUm - EK20 #1202XXXX Pale Mineral Oil '(Extra Heavy White - Sonneborn'e) Barytes - Mepham's #2
20.70#
18. *5 5-85
55-00
#H Aroolor **65 (Code 31*0-01**) 50B Mineral Oil (Extra Heavy White - Sonneborn's)
Barytes - Mepham's #2
#"M" Aroclor **65 Mineral Oil (Extra Heavy White - Sonneborn'e)
#"M" Aroclor **65
Mineral Oil (Extra Heavy White - Sonneborn's) Silica (Schulte, Champlain & Blbbo)
*6.0# *.0
50.0
89.5# 10.5
50-8# 6.8
35-0
For the preparation of thermo-plastlo adhesives Purdue University found that the harder Aroolors are better than anything else dis covered to date, primarily because of their high compatibility with other resins and their thermo-stability.
ELECTRICAL
Dielectrics and Kleotrloal Insulators
The Aroclors have excellent dielectric properties, that is, low dlelectrio constant and resistivity and low power factor. Aro-
clor 12*2 has the highest dielectric constant of the whole series
which we are manufacturing commercially, while higher chlorine Aroolors have higher resistivity.
The Aroclors have found usefulness as a dielectric In condensers and as a dlelectrio and cooling medium In transformersi and a number of miscellaneous similar uses where the characteristics above named are of Importance.
AROCLORS AS SATURANTS
Saturation may be defined as that operation by which liquids or gases ore caused to penetrate relatively parous materials. The penetrating medium Is known as the saturant and is generally In
K0H3AMT0 CHEMICAL COMPANY
10-1-4%
the liquid state. Saturation nay be assisted or aocelerated by means of increased temperature and pressure or by the use of a vacuum.
Various d o s s e s of products are saturated for the purpose of giv ing them a vide variety of properties. Sane of the properties attained by saturation are: water' and flame resistance; resistance to chemicals; abrasion; moisture; light and weather changes; in creased strength; and increased weight.
Among the articles that are treated to obtain some one or all of the above mentioned properties are included the various fibres and fabrics: animal; vegetable and mineral; woods, both hard and soft; c'eramios ware and cement; and certain kinds of electrical appara tus, such as oarbon resistors.
The saturants', or, as they are sometimes called, the lmpregnants, are usually made up of waxes, oils, resins, or water solutions of oortaln Inorganic salts.
Applications
At present the saturating applications that are of chief interest are Insulated wire, low voltage oable commonly called network cable, and oarbon resistor fields. These proposed uses are des cribed more fully under the separate headings which follow.
network Cable
Attempts are being made to develop a use for Aroclor as-a saturant for secondary network or lpv voltage cable. .Cable of this kind Is used in electrical network distribution systems. Oenerally, It
consists of the copper conductor or conductors, the paper insula tion, and the lead sheath. The paper is saturated with an oil., usually a good grade of oil such as the General Eleotrlc Company's Trans11 Oil. This fora of construction Is objectionable because under the conditions Imposed by a short circuit, combustible gases are generated which flow through the conduits to the manholes, at which point they may form explosive mixtures with the air and, In turn, cause explosions in the manholes. Both the paper and the oil are source# of eombustible gases. It Is therefore desirable to replace them -- the paper with an Inert form of Insulation, If possible, and the oil with a non-inflammable saturant such as Aro clor. Thus far, Aroclor 123% appears to meet the requirements of this use.
The more important cable manufacturers In the country are already at vork on the development of a flame resistant cable and also one In vhloh the explosion hazard will be lessened or eliminated.
' 1**i
-
, Mt'n&.aU.:
Monsanto chemical company
10-1-4%
Carbon Resistors
Carbon realatora are email molded rode of a mixture of oarbon blaok and Band with a realnoua binder. They are porous and their elec trical roelstance la seriously afrected by the entrance of molature.
To prevont molature getting Into the unite they are usually impreg nated vlth'some, material to fill up the voids and to coat the sur face of the resistor. A vax le generally used for this purpose and serves very veil as far as moisture-proofing Is concerned. Hovevor, after completion, the resistor must be lacquered for Identi fication. Lacquer does not adhere veil to the vaxed surfaces.
Aroclor 4465 Moisture-proofing Compounds give moisture proofness (Humidity test) equal to that of vax and, In addition, give a sur face to vhloh lacquer vlll adhere.
The Aroclor Compound Is non-cryatalllne and therefore does not have a definite melting point and does not become extremely fluid at the melting point of most vaxes that are used In this application, but it gradually softens under Increased temperature.
In extensive teats to find the moat effective medium for Impregna ting radio resistors to stabilise the electrical resistivity undvr exaggerated and extreme humidity tests, Aroolor 5460 gave by far the best results vhen compared vlth Santovax and various petroleum vaxes and compounds.
This excellent Aroclor success vas accomplished by grinding off or sanding the surface of the carbon resistor prior to Impregnating, thus exposing the Inner pores of the resistor, permitting excellent penetration. Penetration has alvays been a problem In the Impreg nation of resistors vlth resinous materials suoh as Aroclor.
Cable Insulation
Electrical conduitore and cables Insulated vlth asbestos are fre quently lacking In vaterproofness. Impregnation vlth vox canpoeitions gives an Insulating medium resistant to atmospheric moisture and sometimes even to Immersion In vater for a short time, but hitherto no composition having the required characteristics of heat resistance and flameproofness has given sufficient voter re sistance to withstand Immersion for prolonged perlode.
An Improved method of Impregnating asbestos Is described in tJ. 3. Patent 2,162,953, assigned toRockbestoe Products Corporation, vhlch depends on the use of a phenolic resin In conjunction vlth a chlorinated diphenyl. Xt has already been proposed to use each of these substances separately for a similar purpose, but alone the first lacks flameproofness and the second resistance to water.'
.Si-- MONS 092653
MONSANTO CHEMICAL COMPANY
10-1-M
The phenolic reeln used for this purpose should be thermoplastic, solid and rather brittle at ordinary temperatures, with a flow point of 105C. Bakelite XR 8430 Is suggested as a suitable type. The best chlorinated diphenyl for this process is stated to be one having a viscosity of 9 see* Saybolt at 100Ct and, of course. It must mix readily with the phenolic resin. One containing about 62 per oent chlorine Is said to be satisfactory, for example, Arc
elor 1262.
The two Ingredients are mixed In equal parts by weight at 166C, preferably with the addition of 5 per cent by weight of a plasti-
olzer such as Trlcresyl Phosphate. The resulting mixture Is stable and oan be stored.
In manufacturing the cable the individual conductors are Insulated,
twisted and covered with the layers of Impregnated asbestos and varnished cambric (or the like) In the manner well understood In the art. A layer of loosely felted dry asbestos of suitable thick ness Is then applied around the thus assembled cable, and a dry asbestos braid Is applied over the felted layer of asbestos. The so-oovered cable Is then passed through the Impregnating compound (mixture of resinous phenollo condensation product and chlorinated diphenyl) while maintaining the compound at a temperature of about 155C. The time required to Impregnate the layer of felted asbes tos and asbestos braid will depend on the thickness of the layer. As the cable emerges from the heated bath of Impregnating, compound, It Is passed through suitable snubbing devices to remove the excess compound from Its outer surface.
In order to prevent migration af the outer surface compound when the finished wire or cable Is subjected to high temperatures In service, It has been found advantageous In sens Instances to ap ply to the Impregnated layer of asbestos a second coat of the
Impregnating compound to which has been added about 15 to 20J< of
ground mica or other finely divided Inert solid material. The Impregnating compound on the outer surface of the impregnated asbestos then contains dispersed finely divided particles of the Inert solid material which act to thicken the compound and render It less susceptible to flow. The admixture of mica or the like Is not required or desirable In the compound used to Impregnate the asbestos layer, since the asbestos fibres themselves satisfac torily perform the function of retaining the compound within the mass by capillary attraction.
The Insulated conductor or cable of the Invention poaaesses all the necessary characteristics of heat resistance, flameproofness, pliability, dielectric strength and resistance to water. The outer Insulating layer of asbestos Impregnated with a mixture of resinous phenolic condensation product and chlorinated diphenyl Is substantially waterproof, even when submerged In M t e r for ex tended periods of time or subjected to hydrostatic pressure as high as 25 pounds per Square Inch. In general, the ue of asbestos
- 12-
MQNS 092654
. .
____
10-1-M
r
MONSANTO CHEMICAL COMPANY
as an electrical insulating material has heretofore been limited
to locations vhere high temperatures or the hasard of Inflammable
material made the use of ordinary forms of Insulation (such as
rubber, varnished cambric, paper, etc.) undesirable or prohibitive.
It'vlli, therefore, be evident that the invention widely extends
the usefulness of asbestos Insulated wires and oables.
Condensers
A rapidly growing use of Aroclor Is In the manufacture of the small condensers employed In fluorescent lighting fixtures for offices, business houseB and factories.
AROCLOR EMULSION FORMULA
16 pounds of Aroclor - liquid
8 pounds of Water
16 ounces of Stearic Acid
4 ounces of Triethanolamine
The Aroclor is heated to a workable viscosity above 82C (180F)
and the Steario Acid Is added and completely stirred In. The
water is heated to 97C (207F) and the Triethanolamine added and
c
thoroughly stirred in. After both of these operations have been carried out, the Aroclor-Stearlo Acid combination is poured Into the voter mixture while the latter Is well agitated and then the
whole mixture lp processed through a colloid mill. Good results
may even be obtained without the use of a colloid mill, provided
the mixture Is agitated with a high-speed emulsifying stirrer.
FLAMEPR00FER5
The Aroclors are not Inflammable and when mixed in sufficiently large proportion vlth many other materials have rendered the canpie te compound non-inflammable. For Instance, a mixture of about equal parts of Aroclor 2565 and aaphalt gives a resulting compound that will not permit the spread of flame. Wood may be Impregnated sufficiently with one of the higher chlorine Aroclors, such as 4465, that It will pass the most rigid tests now applied to wood which has been treated for flameproofness, such as the tests used by the Forest Products Laboratory and by the Building Department of the City of New Tort.
We have not yet found a market for Aroclor in the field of flame proofing wood because In most cases vhere the wood Is treated for flameproofness It Is used Indoors where It Is not exposed to leaching by rain, so that one of the phosphate salts Is generally used, However, there may be special uses where these materials are not acceptable ap{d where the prlos of Aroclor is justified.'
(
' : V-':
'
10-1-44 M0K3ANT0 CHEMICAL COMPANY
(
There la throughout the country a tremendous market for compounded waxes for all manner of uses. It la very likely that In some of the applications of these materials it would be desirable to havf them non-inflammable. It Is also likely that the incorporation of Aroclor with some other resinous or waxy materials would give other desirable properties. These applications oould probably be worked out In conjunction with companies who are now in the business of , compounding and selling such materials. There are some of these companies In each of our sales territories.
Aroolors 4465 and 5460 are the most likely ones In this application.
Tests are under way to determine the suitability of the substitu tion of Aroclor 1260 for chlorinated paraffin In the treatment of paullns and tentage for use by the Army. This Is for the purpose of producing non-lnflaipmability, Improving moisture resistance, and mildew proofing.
The Aroclors are remarkably stable and their superiority in this respeot to chlorinated paraffin customarily employed for this pur pose le demonstrated In the following results reported by our laboratory.
c
Light Stability Tests In order to be certain that the tests were comparable In every
respect, they were conducted by personnel of the A. French Textile
School, Oeorgla School of Technology, Atlanta, Oeorgla.
The samples used in these tests had been prepared at Anniston prior to this visit. They consisted of sections of klerbolled ootton sheeting Impregnated with compositions as shown In the tabulation below. Approximately 10{f of chlorinated hydrocarbon vas applied to each of the Impregnated samples. The chlorinated paraffin used had the following characteristics: -
e * Cl2
Sp.Or. 25/25C Viscosity 210op
Pour Point
43.15 1.183
I 75 3U3 -8P
As will be noted, several pigments, namely, P2O3 , BbgO^, and
CaCOx, were also applied to the fabric. These pigments were used In tne following proportions:
FegOj - 10 parts PegOj to 8 parts chlorine In the chlor
inated hydrocarbon.
Sb203 - 10 parts Sb^Oj to 8'parts chlorine,
(
CaC03 - 7i parts CaCOj to 10 parts chiorlns.
MONSANTO CHEMICAL COMPANY
10-1-**
In the testa with the pigmented mixtures, the pigment adhered to the surface of the cloth and was not very evenly distributed.
The actual tests made at Oeorgia Tech. Involved exposure for two hours In a Cooper-Hevett lamp cabinet, them conditioning at 70F
and 65Jt H.H. for four hours or longer, and finally testli^ for varpwlse tensile strength by the grab method with a Scott tester. The Cooper-Hevett cabinet had a Uviare (fused quarts mercury arc) lamp aa the aouroe of ultra-violet light. On the basis of dye fading testa conducted at Oeorgia Tech, over an extensive period several years ago, two hours' exposure In the Cooper-Hevett cabinet Is roughly equivalent to 20 days' average outdoor weathering. This relation does not necessarily apply to tensile strength deteriora tion tests. Judging by the deterioration of the tensile strength of unimpregnated samples, it would appear that 2 hours' exposure In the Cooper-Hevett vas equivalent to much more than SO days' out side exposure.
Summarised data for the tensile strength tests were as shown In the following tabulation:
Impregnation Mixture
Tensile Strength (X)
Unexposed
Exposed
Wo.no (Plain d o t h only)
Chlorinated Paraffin
M
II
ft Pe203
ft 3b203
ft CaC03
Aroclor 125**
ft Pe203 ft 3b203 ft CaC03
Aroolor 1260
ft Fe203 ft Sb203 ft CaC03
55-75
57.75
60.9
57.0 57.9
5*.5 60.1 56.2 53.75
59-^ 58.0
62.*
59.25
27-9
13.1 17 75 '17.5
18.5
2*. 0 27.1
2*.5
25.9
25.75 30.1 3*.9 30.9
A r o d o r 54*2 II H
ft Pe203
ft Sb203 w
ft CaC03
60.1
65.5 63.9 62.*
33.5 3*.l
*0.6 * 0.9
(X) Units aro in-pounds and, except for three Instances, the
values shown are averages of * tests, -
S
, ,,.
. . *iT-
The conclusion from these tests vas that the Aroclora contributed little, if any, to the deterioration of tensile strength of the d o t h upon exposure to ultra-violet light, whereas chlorinated paraffin did appreciably accelerate deterioration under the same
,,.v
HONS 092657
10-1-44
r
MONSANTO CHEMICAL COMPACT
conditions. Also, under the conditions of these tests, all of the pigments tried decreased to some extent the tendering effect of
the ultra-violet light. This is probably not abnormal, sinee the pigments should have reflected a portion of the light rays.
It has been reported that certain pigments decrease the heat sta bility of ohlorlnated paraffin, thus accelerating tendering of treated cotton goods upon exposure in hot climates. Beat stabil ity tests on all of the impregnation mixtures tried as outlined above are nov being run in the laboratory at Anniston.
Compared vith plain cloth unexposed (100$) the hydrocarbon treat ments alone effected the folloving Improvement In tensile strengths
Chlorinated Paraffin Aroclor 1254 Aroclor 1260 Aroclor 5442
7.5^ . 1 . 3 )t
1 0 .5)<
11.8)6
This increase in tensile strength through impregnation is compen sated for in the folloving calculation.
When the "Exposed Tensile Strength" is expressed as per cent of "Unexposed Tensile^ Strength" the folloving relationship is evident:
Untreated Cloth
Chlorinnated Paraffin ft Fe203
it
ft Sb203 k CaC03
ArocIIlor 12II54
It
n
It
Aroclor 1260
II
II
II
k Fa203 k Sb203 k CaC03
k Fe203 4c Sb203 ft CaC03
Aroclor 5442
ft Fe203 ft SbS03 ft CaC03
Per cent Resistance to Deterioration on Exposure
to Ultra-violet Light
51.9
28.10
29.15 31.40
31.52
44.05 45.10
43.62
44.19
43.36 . 51.86
56.00
52-10
*
55-70
52.05
63.53 *
65-53
(
The advantage of the Aroclors in comparison vith Chlorinated Par affin as a non-inflammable, waterproof lmpregnant for cotton fab
ric as measured by resistance to loss of tensile strength on
-16- '
MOMS 092658 '/r.
MONSANTO CHEMICAL COMPANY
10-1 *4
exposure to ultra-violet light Is expressed In the following re lationship, basis equivalent Chlorinated Paraffin treatment as 100*;
Per cent Improvement In Resistance to Deterioration
over Comparable Treatment with Chlorinated Paraffin
Aroclor 1254
"
" * Fe203
"
" A Sb203
"
" A CoC03
Aroclor 1260
If R n
w
n n
A Fe203 A Sb203 A CaC03
Aroclor 5442
"
" A Fe203
"
" A Sb203
"
" A CaC03
Average Average Average
56.7 54.7 42.1 40.1
54.3 77.9 78.3 65-3
98.2
78.6 102.2 107-9
48.4 68.9
Heat Stability Tests
These tests were made by absorbing and titrating the HC1 evolved from 20 grams of chlorinated hydrocarbon when held at 175C and
blown with air at the rate of 0.01 cubic foot per minute for four
hours. This Is the method outlined on pages 375-378 of the Aug ust 30, 1943, Issue of the Amerloan Dyestuff Reporter, Vol. 32, No. 18. James R. Redmond, Textile Technologist, Jeffersonville, Q.M. Depot, was the author of the article.
Data for the tests that have been completed were as follows:
Chlorinated Hydrocarbon Composition
% HC1 Evolved In 4 hrs at I75c
20 amis. Chlorinated P a r a r r m
20 gms.
"
20 gms.
*
"
f. 2.0 g m s , Fe203
*
f 10.5 gms. Sb203
20 gms.
"
/ 6.3 gms. CaC03
20 gms. Aroclor
20 gms.
"
20 gms.
"
20 gms. "
12fl54 M
tt
f. 2 gms. Fe203 2 gms. Sb203
/ 2 gms. 0aC03
0.4l 20.00
0.29 .0.29
0.00 0.01 . 0.01 : . 0.02
MOMS 091459
10-1-44
(
MONSANTO CHEMICAL COMPANY
Chlorinated Hydrocarbon ______ Composition______
# HC1 Evolved In A hr e . at 175C
20
20
20 20
gms. gms. gms. gras.
Aroenlor
ft
M
12n60
ti it
A ? gms. Fe203 / 2 gms. 3b203 A 2 gms. CaC03
0.002 0.02
0 .0 0 5
0.01
20 20
20 20
gms. gms.
gms. gms.
Aroenlor
n
n
5*ti*2
rr M
/ 2 gms. 7e203 A. 2 gms. Sb203 A 2 gms. CaC03
0.00 0.00 0.02 0.02
These data clearly demonstrate the markedly superior heat stability of the Aroolors as oompared to chlorinated paraffin. Particularly significant Is the accelerating action of Fe203 on the decomposition rate of chlorinated paraffin. No such accelerating action was noted with the Aroclors.
While in moot of the testa with the Aroclors our titrations Indi
cated the evolution of HC1 ranging up to 0.02$, the titrations were
so small as to possibly be within the range of experimental error.
At any rate, wo are quite sure that 0.02# HC1 evolution represents
the maximum HC1 loss under the conditions of the tests.
(
Chlorinated Hydrocarbon
f HC1 Evolved In
_______Mixture ______
4 hre, at 175C
20 gms Chlorinated Paraffin and 2 gms Zinc Borate #316?
20 gms Aroolor 1254 and 2 gms Zinc Borate #3167
12 gms. Aroolor 5442 and 8 gms. Tricresyl Phosphate
12 gm s . Aroelor 5442 and 8 gms, Tricresyl Phosphate and 2 gms. Fe203
12 gms. Aroelor 5442 and 8 gms. Tricresyl Phosphate and 2 gms. 3b203
12 gms. Aroolor 5442 and 8 gms. Tricresyl' Phosphate and 2 gms. CaC03
12 gms. Aroelor 5442 and 8 gms. Tricresyl Phosphate and 2 gms. Zinc Borate #3167
15-6 0.01
0.02 0.00 0.01 0.00 0.01
Again it will be noted that the Aroclors are far more stable than Chlorinated Paraffin lh the presence of Zinc Borate,
........
. HUNS 09Z660
10-1-**
^
MONSANTO CHEMICAL COMPANY
HEAT TRANSFER MEDIUM
Aroclor ha# been used for a number of years at Anniston as a heat transfer medium. It Is now employed as such In the HB-*0 plant.
Company (075050) used Aroclor as a heat transfer modiurn in main taining a molten lead bath In vhleh they soaked 1* inch armour plorolng projectiles. They operated one unit using Aroolor and another using Dowtherm. Both of these units were used for several ' years. They then discontinued the use of Aroolor after discover ing corrosion In the Aroclor system, which did not occur In the Dowtherm system.
A company developed some equipment for heating pyrites In which they Intended using Aroclor as the heat transfer medium. Since the equipment was never sold commercially, none of these units involving Aroclor are now In operation
Many people considering Aroclor as a heat transfer medium gave it up either because it would not stand the temperature they required, or on account of fumes coming from the Aroclor, or because It cost more than oil normally used for this purpose.
^
Favorable features to the use of Aroclor for this purpose are:
1. Liquid at room temperature.
2. Does not oxidize,
3. Has nearly twice the speciflo heat of petroleum oils generally used for this purpose.
*. Non-Inflammable.
HYDRAULIC FLUID
Company (576,*50) operating a high pressure steam-electric gener ating plant use Aroclor 12*8 as an hydraulic medium In their gov ernor system. They do not use it as' h lubricant. The Aroclor le used Instead of oil, merely because of its non-inflammability. When oil Is used In the governor system, It' la customary to use the same oil reservoir, both for the lubricating and governor systems. When Aroclor is used In the governor system and petroleum oil In the lubricating system, it le necessary to segregate the two sys tems and use separate pumps for the lubrloatlng and governor sys tems .
Westlnghouse have been the principal promoters of the use of Aro
olor In the governor system as a result of having the oil In a
(
governor system catoh fire In one of the CTefecy Central Light and
Fower Company's stations while Westlnghouse engineers were working
with the unit.
... ,,... .
. ,
'
HONS 092661
'-'
`r:
$f*. .1.
10-1-44 MONSANTO CHEMICAL COMPANY
(
ENAMELS
Company {104460) has obtained some Interesting results with bakedon enamels containing Aroclor 1254, Acrylold Resin and Trleresyl Phosphate, pigmented with Titanium Dioxide and Zinc Oxide. The enamel is baked on at 135C (275?)- They have found that Trloresyl Phosphate aids the Aroclor on baking, giving a hard surface.
This same company has found that mixes of Aroclor and Vlstanex (No. 6 B-80 and B-100) or Aroclor and Vlxtac (No. 1 and No. 2) glvo Interesting properties somewhat like shellac. They state that these produots have good adhesion.
LACQUERS
We have a very good general line-up on the use of Aroclor In laoquers In the booklet P-115 which we have published for distribu tion. This booklet gives the limits of compatibility of Aroclors 1254 and 1262 in Nltroosllulose lacquers. Since this booklet has boon published, a number of companies have started using Aroclor 1242 In special flexible lacquers, such as are used on high ten sion cables, etc. The compatibility limits of Aroclor 1242 are higher than those of the higher ohlorlne Aroclors so that It Is possible to Incorporate enough of the Aroclor to give It extreme flexibility. You have the formula for Aroclor Lacquer No. 34 which glvos the details of the use of this Aroclor In cable lac quer.
The work done In our laboratory using Aroclor In lacquers lndicatss that we get somewhat less chalking with the Aroclor lacquers than with those made up by other formulae. We get practical free dom from checking and cracking and, we believe, better color re tention In the vhite and light colored lacquers. These are Impor tant considerations In lacquer manufacture, and Aroclor should be given muoh more consideration from now on for general use such as an automobile lacquer, etc., than It has received In the past because of the rising prices of other resins which are generally used.
We have a number of customers who use Aroclors 1242, 1254 and 1262
In the manufacture of lacquer.
Lacquer Formulation Chart
Non-Volatile Constituents
1. A resin 2. Nitrocellulose (cellulose nitrate) 3. A plasticiser or softener
' -20'...
't
V'y-
092662 HO***
MONSANTO CHEMICAL COMPANY
10-1-**
Volatile Constituents
1. The alcohol constituent 2. The ester constituent 3. The hydrocarbon constituent
Finished Lacquer
X per cent of the non-volatile (100 - X) per cent of the volatile
The percentage X, of the non-volatile or film-forming constituents,
may vary betvoen 20# and 30# of the veight of the finished lacquer
Non-Volatile Constituents
As has been shown by the table, the non-volatile components of a
lacquer consist of a resin, cellulose nitrate and a plasticiser or
softener. For the rosin, some one of those of synthetic origin
may be employed, or a natural resin such as Gum Dammar may be used. Oum Dammar Is a generally used resin in lacquer formulation, and It
can be taken as the number one component. The number two component is the cellulose nitrate Itself. It is also lenovn as Nitrocellu
lose, Pyroxylin and "PX." To the Industry in general It is "cotton.1
It can be purchased in two kinds, the AS and RS grades. The latter grade Is the one that Is chiefly used by lacquer manufacturers.
The initials Indicate a difference In the method of manufacture,
AS meaning that the cotton Is alcohol-soluble, and RS meaning that
it Is regularly soluble.
Both grades are usually bought wet with denatured alcohol. The viscosity of the cotton is another detenslnlng factor with regard to Its use. The cotton that.is commonly employed by the Industry has a viscosity of one-half second and la known as "half-second cotton." For the third component dibutyl phthalate, trloresyl phosphate or castor oil may be used.
At this point an explanation of the terms "plasticiser" and "sof tener" becomes necessary. The average lacquer technologist uses these terms synonymously, and for this reason they have come to mean almost one and the same thing in this Industry. Strictly
speaking, a true plasticiser should be a solvent for tbe "cotton"
and the resin. In addition, It should have a lov vaporisation loss and should confer such properties as flexibility, pliability, and durability on the lacquer film. Both dibutyl phthalate and trlcresyl phosphate meet these requirement*, Castor oil, on the other hand, does not. In that It Is only a partial solvent for "cotton." It does, however,'give to the film the qualities al ready mentioned, In short. It exerts a softening effect - hence the name "softener." The difference,'then, between a plasticiser and a "softener" is that the former ia,a true,solvent,for the
HONS 092663
MORSAUTO CHEMICAL COMPARE
1Q-1-M
non-volatile constituents of a lacquer, vhlle the latter Is a non-
solvent, or, at best, only a partial solvent. Castor oil is typi
cal of this latter class and is widely used as a lacquer "softener."
Volatile Constituents
The volatile constituents fora what la known as a balanced solvent mixture, the purpose of which is to be used as a solvent or thinner for the non-volatile constituents. The components of this mixture must be in such a proportion to each other so as to Insure a uni form evaporation rate when the lacquer film dries, and also to make sure that no precipitation of the "cotton" will occur at the time of thinning.
The number one, or the alcohol, component is generally composed of ethyl alcohol - 95$ and butyl alcohol. The ester component is made up In general of ethyl acetate and butyl acetate, vhlle the hydro carbon component usually consists of some compound such as toluol or, for special lacquers such, as cable dopes, benzol.
Finished Lacquer
The finished lacquer Is prepared by taking a given weight of the non-volatile constituents and dissolving them in a given weight ci the volatile constituents.
Competition
The question of competition will have to be viewed from two angles; first with regard to the Aroolors as resins, and second with regrr.l to them as softeners. Since the Aroolors have more the properties of softeners than of resins, the softeners are nearly competitive with the Aroclors than are the resins.
Competing Basins - Synthetlo
Name
Number
Manufacturer
Amberol
801
The Beslnoue Products & Chemicals
Philadelphia, Pennsylvania
Bakellte
XB-502
Bakellte Corporation New York, New York
Beckaolte
(111) (inO
Beck, Roller it Company, Inc. Detroit, Michigan
Olyptal Levied
1202'
If!
General Electric Company Schenectady, New York
John D. Lewis, Inc. Providence, Rhode Island
-22-
*ONS 09 2`>`><*
MONSANTO CHEMICAL COMPANY
10-1-44
Competing Regina - Synthetic
Name
Number
Manufacturer
Paraplex*
The Resinous Products & Chemicals Oo. Philadelphia, Pennsylvania
Rezyl
(ill
American Cyanamld & Chemical Corp. New York, New York
Rezyl Balsams -
American Cyanamld & Chemical Corp. New York, New York
Teglacs
-
American Cyanamld & Chemical Corp. New York, New York
Paraplex can probably be considered a softener as well as a resin.
Competing Resins - Semi-Synthetic
Name
Number
Manufacturer
Ester Oum
None
(One of the most generally used resins.)
There are many manufacturers
Natural Regins
Oum Dammar
(Batavia) (Singapore)
Imported - obtained through brokers
Competing Plasticizers or Softeners
Name_______________ Orade_______ Trade Name______Manufacturer
Dibutyl Phthalate*
Monsanto Chemical Co. St. Louis, Missouri
Trlcresyl Phosphate* -
Monsanto Chemical Co. St. Louis, Missouri
Kronltex
Kavalco Products, Inc. Nltro, West Virginia
Llndol
' Celluloid Corporation Newark, Nev Jersey
Abalyn ,
(A rosin product recommended for lacquer formulation)
Hercules Povder Company Wilmington, Delaware
-23-' - ; - V '-
MONS 092665
MOHSANTO CHEMICAL COMPANY
10-1-41*
(
Competing Plasticizers or Softeners
Name________________ Qrade________ Trade Maine_______ Manufacturer
ABM-100
(A modified linseed oil for lacquer formulation)
Archer-Daniels Midland Ccx Milwaukee, Wisconsin
Castor Oil (Baker's)*
Number 4 Rumber 15
Humber 10
AA
Blown The Baker Castor Oil Co. Blown Jersey City Mew Jersey Blown Unblown
Spencer-Kellogg Oil
(A modified castor Spencer-Kellogg A Sons oil for lacquer Buffalo, New York formulation)
Vhere are other manufacturers of these products - this list Is by no means complete.
In listing these products, only those that are In more or less gen eral use have been Included. There are some notable exceptions, however, In the cases of such materials as Abalyn, ADM-100 Oil, and Spencer-Kellogg Oil.
i
The materials listed In these tables must not be thought of en
tirely as competing products because they may be more Important
as aids or auxiliaries In co-development work with the Arodlors.
In fact, It Is believed preferable to regard them more In thle
light than as competitors.
Advantages
In thinking of any advantages the Aroclore may have, the statements made In the final paragraph under "Competition" must be borne in mind. It Is preferable to confine oneself to a discussion or the outstanding properties of the Aroclore, for It le believed that It Is only through the development of some specific property that progress is going to be made.
The properties of the Aroclors thot should be emphasised are:
1. Low vaporization loss 2. Pale oolor . 5. Adhesion 4. Chemical Stability
a. , to light
b. to water, aclde and alkalies
c. to heat
(
d. to oxidation a. to chemical action In general
hONS 092666
MONSANTO CHEMICAL COMPANY
10-1-44
5. Non-Inflammability
6 . Non-corroelvenesa 7 . Solubility in commonly Used looquep solvents
A resume of the properties that Aroclors impart to lacquers and the types of lacquers for vhlch they are recommended may be given briefly as follows:
In a Dammar-type laoquer the plasticiser-softener combination, such os the usual dlbutyl phthalate-costor oil combination, may be advantageously replaced by an Aroclor alone. Tho resulting lacquer is less subject to checking and cracking on outside ex posure and retains its gloss.
Aroclor 1262 may also be substituted entirely for the resin in certain types of lacquer. The clear lacquer, so produced, is practically colorless and provides an excellent base for white enamels. Such enamels, however, do not withstand weathering as well as those containing Dammar in addition to the Aroclor.
The advantageous properties of the Aroclors in Imparting added weather resistance to properly formulated lacquers may be traced to their resistance to the action of sunlight, to their perman ency in the film, and to their extreme ehemioal stability. The Aroclors do hot oxidise, "dry," or harden. The Aroclors are un affected by dilute a d d s ' a n d even by hot oauetic solutions. They are not subject to polymerisation, rancidity on* other change, as far as is known.
When added to a nitrocellulose solution, the Aroclors reduce the vlsoosity slightly. This change in viscosity takes place at once and no further change due to the presence of the Aroclor occurs on several months' aging in closed containers.
By virtue of their high refractive index, they impart apparent depth to the lacquer film. Aroclor 1262 has adhesive properties and the lacquers containing it have good adhesion. Lacquers con taining the Aroclors dry normally and give a hard, non-tacky, durable film of excellent gloss-
Certaln laoquer technologists have found that a lacquer contaifi^g Aroclor can be polished with a minimum of rubbing and, furthermore, that the Aroclor seems to Impart a harder finish to a lacquer film than oils, trlcresyl phosphate, or dlbutyl phthalate. It has also been reported that properly formulated lacquers containing Aroclor show no tendency to "spew" or "sweat out" when buffed.
In addition to the properties of general interest,: other proper
ties of tho Arocloro arc of V-.lue in formulating lacquers to fit
special requirements. Aroclors 1254, 4465, 5460 and 1262 do not
support oorabustion, and when present in nitrocellulose films they
> -25-
m ons 092C<>7
MO1AUTO CHEMICAL COMPANY
10-1-44
retard the rate of burning. The Aroclore retard the rate of trans fer of moisture and of gases through a nitrocellulose film, and by virtue of this fact have already found extensive use In protective lacquers for application over those types of electrical Insulating materials, such as rubber, that deteriorate rapidly In contaot
vlth oxygen, 02one, moisture or other vapors.
Procedure
Upon visiting a lacquer company, every effort should be made to ,
see the chemist In oharge of formulation or production. In large
companies the director of research should always be seen. As a
general rule, a great deal will not be accomplished until these '
respective individuals are seen.
[
A complete discussion of the properties of the Aroclors should be given, emphasis being plaoed upon the possible formulation of a new lacquer vlth some one of these properties ae the background.
When discussing the use of Aroclore In lacquers, the salesman Bhould remember that the Aroclore are not solvents for nitrocel lulose and that for this reason an excessive amount of Aroclor must never be used In the formulation of a lacquer.. The limiting percentages that can be used for successful results have been carefully worked out by a large number of experiments. The few simple rules that must be followed In formulating lacquers with ths Aroclors are emBoJled In a booklet entitled "The Properties of Two Aroclors of Special Interest to Manufacturers of Lacquers." Copies of this booklet may be had on application to our sales offices. It Is recommended that the salesman offer copies of thJ s booklet and the bulletin "Plasticisers A Resins - Organlo Division" to Interested lacquer manufacturers.
Attempts should be made to determine what particular lacquers a manufacturer specializes In and what problems he is studying at tbe time of the coll.
Aroolors have fair or good compatibility with nitrocellulose, Forravar, Butvar, vinyl copolymers, polyvinyl acetate, poly-etyrene, chlorinated rubber and ethyl cellulose. In general, the liquid or semi-solid Aroclors act like true resins. One principal value la their chemical Inertness. Where great flexibility IS to be ob tained, it may be necessary to employ auxiliary plasticizers. 3onu of the exceptions are In chlorinated rubber and in ethyl celiuloee where flexibility or hardness may be varied simply by selecting an Aroclor of the proper physical characteristics.
The liquid Aroolors such as 12k?, 1248 or 1254 will greatly In crease flexibility but will cause softness. . The semi-solids such as 1260 or 5442 will Impart seme flexibility Without the marked softening effect. The brittle, resinous Aroolors such as 4465 or 5460 produce very hard compositions vlth excellent adhesion and
-26-
MUNS 092668
T
' MONSANTO CHEMICAL COMPANY
10^1-44
weathering qualities. If a single Aroelor does not impart the de
sired combination of properties, usually some mixture of Arociors
will do so. It vould seem that in polystyrene molding composl,
tlona, the resinous Arociors could be used as a flux or flow pro
moter at molding temperatures without causing softness and flow, at
normal temperatures. Some mixture of Arodors or a combination'
of an Aroolor with another plasticiser either solid or liquid
might be required for this purpose.
'
Of course, it is well known that for alkali resistant coatings, . combinations of Aroolore (1254-1260 and 546o) with chlorinated rubber have been used for a long time. At the present time, the use of equal parts of Aroelor 5460 and ethyl cellulose is being pushed by Company (331850) as a weather resistant coating. Sim ilar coatings of low vleooslty polystyrene and Aroclors would probably be of value.
ARMY-NAVY AERONAUTICAL SPECIFICATION LACQUER - CAMOUFLAGE
AN-L-21 8 October 1943 - Page 14
TABLE IV
Control Formula - Clear Vehicle
Weight
Weight
lbs. per
Ingredients
Percent
100 gal.
Volume g a l .per 100 gal.
Paraplex RO-2
Uooj<) 11.1
90
.
Amberlac B-94
(80)G in xylene ) 5,6
45
Arcelor 5460
(100j<) 4.3
33
.
Ethyl Cellulose (3 to 4 s e c H 100#) 4.3
35
,,
(1/4 sec.R.S.)
Cellulose-Nltrate/gcg lh ethyl' 9.4
75 '
-
alcohol)
Ffryl Alcohol Eth/1 Acetate
. :?.5
.. .. ^ _
4
4.5
_
5
Butyl Alcohol
- -
12.4
15
Butyl Acetate
22.4
25
Aro;.i.itlc' Petroleum Naphtha Type 1, Grade B
...gg-5-;.
....-- ?5''
:.-i.... .:.Um1'.,...,-'.., *
i
n., MONS 092669
' .... ...
-27, ...
.
!U -
i i A r - !? .* * ., ' to n .Siw SsafiM iW lisisaigW pIn IilliBETSI
W
10-1-44 MONSANTO CHEMICAL COMPANY ( It Is also of value In other resins uhere a highly alkali re sistant plasticiser Is required. Papers by Bovran, Paint Technology (reference for December 1936, dated January 1937) Indicate many possible applications for the Aroclors. Sales to lacquer trade at present are oonflned to specialty manufac turers.
The compatibility of Aroclor 4465 In 1/4 second nitrocellulose is Indicated as:
1. Between 24.2# and 26.5# by Inspections for blush In thin aged films.
2. Between 13.7# and 16.6# by inspection for loss of gloss In thin aged films.
The presence of a mutual solvent such as dibutyl phthalate raises the compatibility.
The formulation of a Tlexlble lacquer designed for oven drying Is given as follows:
(15-20 Sec. R.3. Nitrocellulose 32#
Non-Volatile 25# (Tricresyl Phosphate
4o#
('
(Aroclor 1242
28#
Volatile 75#
(Benzol (Alcohol (Ethyl Acetate
62# 22# 16#
This formula 1b intended for application followed by oven drying. Air drying at atmospheric temperature causes blushing. A modi
fication of the volatile portion Is suggested when air drying Is used.
Volatile
Alcohol' Ethyl Acetate Butanol Butyl Acetate Toluol
6.4# 6.4# 6.4# 30.8# 50.0#
Experiments on flock Insulation and lacquers for aircraft Indi cated Tricresyl Phosphate as a choice over Aroclors in Ethyl Cellulose lacquers, especially since there Is no tendency to settle out when Tricresyl Phosphate Is used. Aroclor Is more effective In flame retarding, however.
Stop-Off Lacquers
Rather detailed Information is given In the Monsanto (Organic Products Division) Plasticizers and Resins Booklet on the prep aration of Nitrocellulose lacquere containing Aroclors. A
vaft"'IT'.
' ^ . ` "..4 mqnS 092b70
MONSANTO CHEMICAL COMPANY
10-1-M
(
suggested formulation Is as follows:
1/2 second Nitrocellulose, Dry Aroclor 1260 Trlcresyl Phosphate Santlolser B-lo may be substituted for
Trlcresyl Phosphate
100 80-70 39-70
If the Nitrocellulose Itself does not have sufficient resistance, a composition of Aroclor with a chlorinated rubber, Ethyl Cellu lose or a Vinyl Resin again using Aroclor Is suggested, and If the flexibility Is not sufficient, It can be Improved by the ad dition of a small amount of one of the liquid Aroolors such as
12*12 or 125*, although again Trioresyl Phosphate or Santlclser
B-16' could be used.
In coatings, as a general rule, the hard resinous Aroclors will produce very hard and very resistant compositions, but these will be brittle. The liquid Aroclors will tend to produce flexibility but may be lacking somewhat In adhesion. It Is for that reason that we have suggested Aroclor 1260, which Is about half-vay between and will produce a combination of flexibility and adhe sion. It will be' obvious that hardness can then be Increased by the addition of a harder Aroclor such as 5*60 or the flexibility, can be Increased by thS use of a liquid Aroclor. The Aroclors themselves are unaffected by acid and alkali.
Stop-Off Waxes
The characteristics of a stop-off wax should be as follows:
a. Tightly adherent to metal surfaces. b. Should not be removed at a bath temperature of 160P. c. Should not be'affected by the acids or alkalies of
electrolytic baths. d. Should prevent eleatrolytlc activity on the surface
covered. e. Should be capable of removal by solvent vapor phase
cleansing baths, by melting in boiling voter, or ordinary cleaning solutions.
Suggested compositions are as follows:
Methlde (Monsanto Merrlmac) Aroclor 5**2
Methlde (Monsanto'Merrlmac) Aroclor *A65
* 0* 60* 20* 80* -
Softening Point 118C.
108C.
An attempt was made to use these compositions In solution form by dissolving them In turpentine. This was not particularly
. Y,,';'
^
'Aif
-89- .
oltf
HONS 092671
HOBSAHTO CHEMICAL COMPANY
10-1 -M
successful since at room temperature the degree of solubility was lees than 12$. It might be possible to use a 25$ concen tration of wax In turpentine at 50-75C pointing the metal J surface with the hot solution.
PAINTS
Paints containing Aroclor have shovn remarkable durability*for better than any other .paints against vhloh they vere tested.
One serious drawback, however, Is that paints containing Aroclor do not brush as readily as the normal house paints. Paint manu facturers Interested In quick drying paints should be encouraged to try Aroclor. Under war conditions there le great interest in the manufacture of fire-proof painting for the Interior of ships Aroclors should be a definite contribution to their formulation.
Aroclor 5^60 is euooeesfully used In camouflage paint where It Imparts flameproofness.
VARNISHES
There has been only a limited amount of work done In our labora tory on the subjeot of Aroclor In varnishes and from that work it has been concluded that the moet likely field for Aroclor In varnishes Is In conjunction with some other resin such as Ester Oum or Dammar, or one of the other commonly used gums, since the use of Arqolor alone has. In our experience at least, given a tackiness to the film.
Aroclor 1262 mixed vlth Bast India Oum and cut with naphtha fur nishes a varnish base.
The Aroclors may be used In alkali-proof varnishes by Incorpor ating them as a cold out or as a chill hack -- and for the pur pose we recommend Aroclor 1262, The Aroclor may be said to function either as a resin or as an oil. In other words, by the addition of the Aroclor, a short oil varnish takes on many of the physical characteristics of a long oil varnish. Our work along this, line has Indloated that the best procedure Is to cook (In the usual manner) using as a resin base a pure phenolic resin hut using only half the usual amount of china-wood oil, When the varnish attains proper body, the Aroolor may be added directly as ohlll back and the varnish then thinned iq the usual manner.
Since Aroclor 1262 le s'semi-solid resin, It Is best heated until liquid before Introducing as the chill back.
An optional method is. to dissolve It In the thinner and add In the usual thinning operation. This was worked out a* a possible means of extending the suppllesof china-wood oil. In other words. It acts as an.oil .substitute more than ap. a resin sub-.. stltute
HONS 092672
MONSANTO CHEMICAL COMPANY
10-1-44
In regard to the alkali resistance, ve have found that provided the other materials have, of themselves, considerable alkali resistance, then the Aroclor will add to that resistance. It Is not possible, however, to use a resin such as limed rosin or ester gum having poor alkali resistance and Impart high alkali resis tance by the addition of the Aroclor.
Aroclor 1262 can be used to replace up to 50 of the china-wood oil in varnishes.
1. If ester gum, rosin... or other cheap resin Is used, the varnish will be suitable only for Interior work.
2. If a good 1000 phenolic resin Is used, the varnish will be satisfactory for exterior purposes.
Varnishes containing Aroolor 1262 are not superior in quality to similar varnishes made with tung oil alone, with the possible ex ception of a very slight improvement In alkali resistance, flexi bility and adhesion In some formulations.
Varnishes containing Aroclor 1262 soften at lower temperatures 'than do varnishes employing only tung oil, and'so are more sub
ject to "printing" and marring when warm.
The advantage of Increased flexibility of Aroclor varnishes Is lost, at low temperatures due to embrittlement of the Aroclor.
Because Aroclors weigh more per gallon than china-vood oil, they Increase the cost of varnishes (which are sold by the gallon) even if put at the same price per pound as the oil.
LUBRICANTS
An outstanding service Is performed by Aroolor 1254 as a lubrloant for high pressure air compressors operating at 4400 pounds per square Inch pressure. Besides avoiding flammability, It Is claimed that the lubricant is superior to oil, no corrosion de posits result, and there Is no exoesslve vear on the equipment (Company 15850).
Company (233960) Is using Aroclor In a special drawing compound. Company (541370) tested Aroclor 1248 lri one of their pumps operat ing at 2500 pounds pressure with the following results: .
Compressibility change Is 0.50 compared to 0.50 for petroleum oil.
The vear rate of the pump was measured by observing the slip of
the pump at intervals during the enduranoe run. Inspection of the
pump shoved the wear, to have occurred on the. piston hole walls In
the cylinder and on the hardened surfaoe of the pintle, the sur
face of the pintle felt wavy - not smooth.' A wear rate'of 220 per
1000 hours was found to exist. The viscosity'slope of Aroclor 1248
was poor. .
.
.. .
...
M0NS 092673
, MONSANTO CHEMICAL COMPANY
10-1-4*
The conclusion of these tests is reported ss follows: Aroclor 1248 is not a very satisfactory fluid for general use in oil gear pumps at 2500 pounds per square inch. It is expensive as the pump requires special paint on the Outside and inside; the oper ating range is narrow and the wear rate on the pump tests was 22$ per 1000 hours at 100F and 25 pounds pressure.
Our experimental work in using Aroelor as a lubricant in steam ' turbines was not successful, due principally to the fact that the Aroolor is of such high density that it picks up any bit of grit that may be in the system and floats It up in ^he bearing.
Petroleum oil having so much lover density allovs most of these particles to settle in the bottom of the reservoir.
United States Patent #2,2*5,649, assigned to Celluloid Corporation, describes a steam turbine lubricant consisting of 50 parts of
chlorinated diphenyl and 50 parts,of triaryl phosphate.
- E. P. Lubricants
Much attention is being given by lubricating men to the matter of increasing the film strength or load carrying capacity of lubri cants, particularly so as to be able to use smaller gears for a given load
There are a great many such lubricating compounds now on the market. As a class they are called "Extreme Pressure" or E. P. Lubricants.
It is well accepted in the lubricating Industry that by the addi tions of certain elements as Chlorine, Sulphur and others in the proper form to a lubricating oil, a certain chemical combination takes place with the iron or steel metal bearing surfaces. These surface compositions tend to prevent seisure of the rubbing sur faces under extreme loads and under vhloh loads, if the sole lubricant was a pure mineral oil, seisure or scoring would result
at once through film failure.
In attempting to discuss Aroclor as an extreme pressure base, it is very difficult to evaluate its comparative load-oarrylng capacities with.other extreme pressure bases, such as lead soap, active sulphur, saponifiable oils, sulphur chloride, etc., without sotual results from exhaustive tests not only of the various E- P. testing machines, but also from actual service under normal operating conditions. It is recognized by the lubricating indus try that results obtained on testing machines, such as Almen machine, Timken machine and others, mean very little unless the results are correlated and proved by service conditions. It Is true that in the past Aroclor has been tested'as an X, P. base on the Timken machine at Timken Holler Bearing and on the Oeneral
;
r?~ ri--
092t>74
hqns
MONSANTO CHEMICAL COMPANY
1 0 - 1 -A A
Motors machine at (Jeneral Motors Besearch, and In each case the Aroclor addition has ahovn a marked Increase In load carrying capacity. . '
Several companies are purchasing Aroclor today for use in 8. P. Lubricants, but indications are that they semetime add other elements along with the Aroolor to achieve commercial results at a lower price. Since we have never run service tests on the Aro olor ourselves and the few companies purchasing Aroolor are naturally very reluotant to divulge their experience along with what other chemicals, if any, they are using In conjunction with the Aroclor, the best that can be done Is to offer comments by several of the companies who have tested the Aroclor and possibly give a general Interpretation or suggestions as to where It might find more general present day application.
Top Cylinder Lubricant
Heuently the practice of putting a lubricant In motor gasoline has became quite general. This Is, of oourse, to lubricate the top section of the cylinder.
We have two customers who purchase Aroclor regularly for use In the top oyllnder lubricant, which they make and sell.
We do not know the function of the Aroclor In this use other then that,these customers tell us that it prevents the deposit of carbon on the valves. Ve understand that they use a relatively small percentage of Aroclor in the lubricant.
One of these customers uses Aroclor 1248 and the other uses Aroclor 1154.
We have- done very little work with the Aroclor as a top cylinder lubricant but would suggest that Aroclor 1248 be used In small percentages. This Aroolor will be found completely soluble In low viscosity oil and should not cause any appreciable difference In its cold test. This Is often added to the gasoline to achieve top-cylinder lubrioatlon.
Company (735900) obtained excellent results using Aroclor 1254 on a bearing test, operating in straight Aroclor at 255-260P (124-129C) for tvo weeks. Muoh less carbonisation and decom position than with the usual spindle oil under the same conditions.
PLASTICS
Compatibility of Aroolors with Cellulose Acetate
Experimental W o r k . The compatibility limits of Aroclor 1262 were determined with five grades of cellulose acetate, Tor these .
HONS 092675
MOIBANTO CHEMICAL COMPANY
10-1-44
cellulose acetates the limits sere as follows:
Eastman Cellulose Acetate Number
Compatibility Limit of Aroolor 1262 (per cent)
7025 7026
_ 7027 7028
10246
Between 10.0 And 13.6 Between 16.2 and 17.9 Between 13.1 and l6.b Between 17.8 and 19.7 Between 16.4'and ifi.l
These figures, as well as all the compatibility limits given In this report, refer to the limits as determined on thin films dried slowly In dry air and deposited from solutions containing, as Is customary, 0.1 gram of "solids" per cubic centimeter of
solution. The solvent was a mixture of 80$ by weight of ethylene dlchloride and 20jC of alcohol (denatured, Formula 3A).
Another solvent mixture comprising 33.3# acetone, 33.3J6 ethyl lactate, 16.756 alcohol and 16.7)6 ethyl acetate (all percentages by weight) was less suitable than the solvent given above, and gave lower compatibility limits in the cases tried.
Tne compatibility limits of several Aroclors with one cellulose
acetate (#10246) were determined. The observed limits were as
follows:
'
Aroclor No.
Limit (Per cent)
1242 1254 1262
4465 5465
From 25.9 to 28.7 From 25.7 to 29.1 From 16.4 to l8.1 From 14.2 to l6.8 From 10,1 to 13.0
The ternary systems, comprising a cellulose acetate, Aroclor 1254, and a common plasticizer, were Investigated.
The constants of the eellulose acetates, 'as given by Eastman
Kodak Company, are as follows:
-.-.y '
.Cellulose
Aeetyl
Acetate H o . (Per cent
Viscosity (Seconds]
MONSANTO CHEMICAL COMPANY
10-1-44
Conclualona
The compatibility limits of various Aroolors In a specific cellu lose acetate and or one Aroclor in various oellulose acetates are comparatively lov. The type of solvent employed affects the ob served limits, *he solvent whloh gives the more favorable results being the mixture of ethylene dlohloride and aloohol. The com patibility limits of the Aroclors in oellulose acetate are. In general, more dlffloult to determine and less readily checked than the limits In nitrocellulose. The actual- observed limit apparently depends upon the rate of drying, the thickness of the deposited film, the humidity of the air, and the solvent employed.
In the tests of compatibility made by Eastman Kodak Company, the limits were found to be 50 to 100 (Rittenhouse). Their lov re sults vere probably due to their method of detecting Incompati bility, In which delicate optical methods vore employed to detect hate In the film.
The work on the effeot of Aroolors upon the rate of burning of cellulose acetate films, as given In the table, leads to the following conclusions:
1. Cellulose Acetate alone' burns slowly.
2. The rate of burning, where burning takes place at all-, is accelerated by each of the substances tried.
3. While the Aroclors Increase the rate of burning, they at the same time give a flickering uncertain flame' vhlch tends to go out, that Is, they tend to quench the flame,
4. Trlphenyl Phosphate Is an effective flameproofer. It be ing Impossible to Ignite the film containing 250 of It.
5. If flexibility and lack of tendency of the film to wrinkle or curl on drying is taken as a criterion of plasticising power, -the Aroclors are more effective plasticisers than either dibutyl phtbalate or Trlcrosyl Phosphate.
6. The thick film containing 250 Aroclor 1254 (slightly below the compatibility limit for thin films) was blushed. This is In acoord with the earlier observations of the effect of film thickness on the compatibility limit.
Company (756593) has found that mixtures of decachlorodlphenyl and styrene are non-lnflassnable and have a heat distortion point 20P higher than polystyrene.
United States Patent No. 2,227,637, assigned to Leverkusen-I.O,
Verk, describes a composition of matter comprising a realn-llke
chlorinated diphenyl of an average chlorine content of about 620
..... ...... .
.r.5... '
HONS 092677
MONSANTO CHEMICAL COMPANY
10-1-44
and about 1.5% of polyvinyl earbasole.
RUBBER
Company (.297400) have found that Aroclor 1262 is the beat plas
ticiser for rubber hydrochloride. It la compatible up to 100J< rubber hydrochloride, although the uaual working range is 5 to 10% of Aroclor 1262 baaed on the weight of the ohlorlnated rubber. Below 50% Aroclor no difficulty la encountered with brlttleneaa. Aroclor tenda to lncreaae the gloas of rubber hydrochloride fllma,
e.g., Pllofonn, Pliofilm, Pliollte. Five por oent rubber hydro chloride added to Aroclor reducea the tack.
On tho other hand. Company (331850) recommends the uae of Aroclor
125*1 with chlorinated rubber, e.g., Parlon.
fiaurr
f
/ (7JU^b s - /
A rubber oompoaltion of reduced flammability comprises
>**.
Rubber Chlorinated rubber Aroclors Sulfur Zinc Oxide Vuloanlclng Accelerator Ammonium Borate
100 parts 35 parts 65 parts
2.8 parts 5 parts 1 part
40 parts
Th]? composition shows a flame resistance'and a notable absence of melting around the burning material.
Aroclor 1268 is used In the manufacture of Cellular rubber of low flammability for the aircraft industry.
Company (284144) has found that 15% of Aroclor 1242 added to
Vlstlnex (polybutene) makes a de-icing coating for airplane pro
pellers that looks promising. By the addition of plasticiser
C-2V or plasticiser SC, low temperature characteristics can be
obtained.
.. ..
it is indicated that Aroclor 1242 may act as a solvent for one of the materials which is producing tack in Buna 3.
The characteristics of Type B Keoprenp compositions are said to be improved by the addition of Aroclor 1254 Increasing water
resistance. (Company 16947) ,
The use of Aroclor 5160 Is under investigation as an extender for Hycar OR.
There are several different applications for Aroclor in rubber
as follows:
-
.
; -vs.,
r
MONSANTO CHEMICAL COMPANY
As a plasticizer for hard rubber
10-1 -44
Aroclor 1262 has been used as a plasticiser for bard rubber In dental plates, eto., for a couple of years. It should be equally useful In plasticising herd rubber for other purposes vhere brittleness Is undesirable.
To render rubber permanently tacky .
Aroclors 1262 and 1254 are milled Into rubber'so as to make a homogeneous compound vhlch has permanent tackiness or adhesion.
To flameproof rubber. Neoprene, and other synthetic rubbers
Aroclor 1269 Is a hard crystalline material of high melting point. It may be ground very fine. This finely ground Aroclor Is milled Into the rubber Just as any Inert filler vould be. The milling temperature Is not high enough to melt this Aroclor and so there la no solvent action. It has been found that the Incorporation of sufficient Aroclor 1269 in rubber prevents the spread of flame. This Is suggested especially for flameproofing rubber for use on Insulated vlre.
THERMOSTATS
C
Aroclor 1248 Is being used by several manufacturers of thermo
stats as the expanding medium In the bulb. Aroclor has been
used In this service by one manufacturer for the last ten years.
Aroolor'has proved entirely satisfactory. Every precaution must
be taken to eliminate the possibility of moisture or other for
eign matter getting Into the Aroolor. The thermostat equipment
must be thoroughly cleaned before filling.
We do not recommend the uBe of Aroclor at temperatures above
600OP (3150c).
TEXTILES
Company (645300) reports that Aroclors^ although more expensive,
exert better fire retardant offeot than chlorinated paraffins
and smaller amounts are required.
....
Company (049900) claimed that Aroclors 1262 and 5460 shoved a 10)1 Increase in tensile strength vhen substituted for the stand ard Jeffersonville Quartermaster Depot specified impregnant for rope, vhloh Is the follovlng formula:
41)1 Copper Naphthenate 800-8 98)1
14)1 Asphalt
' ..
30)1 Paraffin Wax
.
j
15)1 Mineral Seal Oil
10-1-44 NONSASTO CHEMICAL COMPANY (
Aroclor 1260 Is proposed as a flameproofing, waterproofing, mlldewprooflng agent In the production of J.Q.D.'s specification 242 paullns and tentage for army use. Exact formulation'and approval of the Quartermaster Corps has not yet been worked out.
'
WOOD
Aroclor as an Introfler for Sulfur In Wood Impregnation
It has been found desirable for some purposes to Impregnate wood and other fibrous materials with sulfur. However, sulfur does not go Into these materials without difficulty. The use of 10$
of Aroclor 4465 mixed with the sulfur aots as an Introfler, caus ing thorough penetration.
The Impregnation is performed as followst
A mixture of 90$ sulfur and 10$ Aroolor 4465 la melted and mixed I A-
and placed in an autoclave or pressure tank with the wood or other
material to be Impregnated and held at a temperature of 125C to
140C and a pressure of 100 pounds per square Inch. The time
necessary depends upon the kind of wood or other material being
treated. The Initial fredslng point of this mixture Is 107.5C.
,
c
The viscosity at 125C Is reported as 27 Seconds Saybolt Universal. / A typioal impregnation of a yellow- pine 2" x 8" plank gave an
Increase In weight of 127$ and about 100$ in tensile strength.
The valuable qualities contributed by this treatment are added strength, rigidity, resistance to moisture, to acids and to splintering. The electrical Insulating properties are Increased. The wood Is made practically free from the effect of weather and resists attack by lnseots. The treated wood Is practically free from shrinkage and swelling.
Possible uses of wood treated in this way are:
Transmission line crosaarms.'
Tanks to resist aolds, etc.
Equipment In which swelling or splintering Is objectionable.
Timbers likely to be attacked by termites, etc.
Perhaps many other applications where the qualities described above are desirable:
The requirement Is that the wood so treated Should stand being :
l.
used 15 or 20 times In concrete forms, that, it must remain smooth,
and not show annular ring or grain structure' 00 the concrete
MONSANTO CHEMICAL COMPANY
10-1-**
where the forms are used. Plywood Impregnated with a mixture
of Aroclor 2565 and 10-20$ hard paraffin (melting point 60-68C) would be suitable for the construction of concrete forms. Addi tion of suirur up to 200 of the mixture may be beneflolal In reducing the cost of Impregnating material and In making the treated wood harder.
The reoommended procedure'consists of keeping the plyvobd sub merged for 30 minutes In the Aroclor-Paraffln mixture (or Aro clor, Paraffin, Sulfur mixture) at 80-90OC, then letting the
boards drain at about 50C and passing them between rollers to wipe off the excess of the wax.
Plywood treated In this sianner Increases In weight from 37 to 66$
and gains only 3.1 to 5.7$ In weight when Immersed in water for
six hours. Untreated vood gains 29$ in weight when kept In water
for an equal length of time.
Standard maple vood blocks used by the shoe last Industry from (Company 769520) were treated with various compounds to prevent
dimensional change from water absorption. The most effective composition was found to consist of:
70$ Aroclor 2565 20$ Paraffin (hard or soft) 10$ Sulfur '
When this composition was applied under the conditions shown be low the results Indicated were obtained:
Weight of Treatment . mg/sq.in.Surface
Effect of Soaking In Water 24 hrs. ' $ Per-
O a i n l n W t . Imeter g/sq.Heter Change
1.- 60 min. at 100C. 1 ; 30 min. cooling
*5.36
3*0
0.3*9
2. 60 min. at 100C.; 30 min. cooling
*2.96
375
0.3*9
3. 60 min. at 100C.j 30 min. cooling
*. 60 min. at 100C..j .
30 min. cooling
1 '
*9 . 2 6 *9.50
. 351 367
0.3*9 0.525
5. Vac. 30 min. at 90C 5 min.. released 10 min .
Maximum tolerable limit
36.*9 - v;:- .... * 8 7 . , ; 0.175 ...... ,V V 0.556
MONSANTO CHEMICAL COMPANY
10- 1-4*
From another series of tests conducted on hickory fishing pole handles It Is concluded that the best results will be obtained using the following conditions!
Temperature Vacuum Atmospheric pressure
Remove, drain and dry
90-100C 16-100 am. for 25 min. 5 min.
MISCELLANEOUS ...
Purdue University found that Aroclor 1242 was very useful as a base upon which to flow gelatin solutions for the production of films, thus making It possible to eliminate mercury for this purpose.
As a result of Interest aroused In the Aroolors, several sugges tions have been made regarding uses which may prove of value.
1. Aroclor 1260 as an adhesive In a Joint compound for glass building blocks.
2. A water emulsion of Aroolor 1262 for use In leather, paper, textiles, rubber and casein paints.
3. As a protective coating on certain pigments to prevent "llverlng" of paints containing resins of a high acid number. Specifically, sine oxide pigment In water emul
sion of "Aquaplex," a water emulslflable alkyd resin.
4. A waterproofing for concrete.
5. Aroolor 1262 or 5460 as an Ingredient of molding'composi tions made with such materials as ethyl cellulose, bensyl cellulose, soy bean meal and corn protein.
(
MONSANTO CHEMICAL COMPANY
10-1-44
SUGGESTED FORMULAE FOR MOISTUREPROOFING '__________ COMPOUNDS_______ ____
Compound A Compound B Compound 0 Compound D
96.056 Aroclor 5460
4.0)6 Bard Paraffin
96.0ft Aroclor 4465 4.0jf Hard Paraffin
96.0)6 Aroclor 5060
4.0)6 Hard Paraffin
96.0)6 Aroolor 4o65 4.0j6 Hard Paraffin
When a relatively low softening point material la de sired, we suggest those compounds using Aroclor 4465. When a higher softening point Is required, we suggest the compounds using Aroclor 5460.
Compounds C and D are black materials and are useful where oolor Is of no Importance.
Ve do not prepare these compounds.