Document x5GYENLaB8GqO5MROmByNgZqG
SOPTNISS AND FORMATION
Another example ed pipe* properties experienced with Hi|h Purity Atboim additions n illustrated in Table I. Hi*h Purity Asbestos was added to a 30 lb. wet atped towel and softness was found in improve over 20. Additional hcnciit' included improvements is wet tear. * stretch, and an obvious reduction of solid* in the clarified water tt the effluent of the saveall.
TAiiei THAI DATA
Basis Weijht flbs'^'UIS'i**') Softness (Crush Tew 1 Bulk (4 ply cap.) % Stretch Wet Tensile Aged (one inch strip afrd m oven at IM'C tor 10 min.)
Machine Direction On** Direction
Dry Tensile (one inch strip)
Machine Direction Cross Direction
Wetjcir
Machine Direction Cm** Direction
Absorbency (1 1 Occ) Seconds
N* S4mm
30.0 2200 0.267
6.5
2.7 1.7
9.6 5.7
30 34
35
erut MUnw hh FipH
19 - i%
*%
30.1
29 .t
JO.4
1700
1610
16*0
0.2611
0.266
0.274
7.4 7.2 7.1
-- 2.1 2.7 -- 1.5 1.6
-- 9.3 (ft -- 5.5 S3
-- 36 42 -- 42 52
t_ 33 35
Formation improvement* are often dramatic with Hi|h Punty Asbestos addition.
M7059