Document x1o1X3JJqj75jO4600veXEL0Q

STLCOPCB4094953 ml v > 4 ? i- ''4**ii4***fc' at . t; $ II 't DISTRIBUTION Pile R. E. Hatton J. H. Lum - F. B. Zienty - Pile Duplicate File Circulate: Assoc. and A33lst. Rea. Directors T. P. Sands - Organic Division Development Extra Extra . Extra This report contains confidential information which 13 the property of the Monsanto Chemical Company and which shall be disclosed only to duly authorized persons. The recipient is held accountable for the filing and safe custody of the report which must be returned on demand. it i i i~ ' t DSW 620926 f! STLCOPCB4094954 hM f-i '* i 'f- I. INTRODUCTION , II. SUMMARY .......................................................... . ...................................... 1 III. REFERENCES.......................................................................................................... IV. EXPERIMENTAL WORK AND DISCUSSION.................................................... A. Pydraul F9. ...................................................................................... 1. Viscosity Index Improvers ... ............................. 2,3,4,5,6 2. Thermal Stability .............................................................. 6 3. Lubricity Additives ........................................................ 6 4. Other Tricresyl Phosphates.......... 7 B. Pydraul 600........................................................................................... 1. Formulation Studies ......................................................... 8,9,10,11 2. Viscosity Data........................................................................11 --- 3. Solubility of Water inPydraul 600 .......................... 11 C. Pydraul 150........................ ............................................................. ~ 1. Formulation Studies........................................... .... 12 2. Viscosity Data........................................................................12 3. Solubility of Water inPydraul 150..........................13 4. Thermal Stability.............................................................. 13,14 D. Navy Fluids................................................ ..................................... 14 1. OS-54.......................................................................................... 15 2. OS-63........................................................................ .... 15 3. os-66................................................................................. .... . 16 4. OS-70 (Triaryl Phospi_ats)...................................... ,, 1-- E. Pydraul AC (OS -67}....................... ........ ....................................... 16,17 F. Steam Turbine Fluids................................................................... 17 G. L-3A* Fluid........................................... .... . ;.............................17,18 'os-41 X; i.j. HJ M 1 ' .I -- Phosphate Esters :6nc LUS * . DSW 620927 STLCOPCB4094955 Ea IfMh* I. INTRODUCTION Monsanto has been actively Interested In the field of functional fluids since 1948. Two lines of products, Skydrol fire resistant aircraft hydraulic fluids and Pydraul fire resistant industrial hydraulic fluids, have been Introduced and several Individual fluids have reached commercial status. Research has continued on both the new fluids and those m the research and development stages. This report covers work on functional fluid application research principally in the Industrial field and Includes formula tion studies, property determinations, and sample preparations. The period covered by this report 13 from August, 1954 through December, 1955. II. SUMMARY The Pydraul series of fire resistant Industrial fluids was extended to include Pydraul 150, a low viscosity, low temperature fluid, Pydraul 600, a high viscosity fluid, and Pydraul AC, an air compressor lubricant, as well as Pydraul F9, a medium viscosity fluid. Formulation studies were carried out and tentative processed developed. Acryloid 710 was adopted as the viscosity index improver for this series wherever needed replacing Santodex which was with drawn from the market. Physical and chemical properties were studied for these Pydraul fluids and for several development fluids. ' Cooperation was given in the Navy's search for fire resistant shipboard hydraulic fluids by provision of new fluids. Samples of a fire resistant steam turbine lubricant, an adhesion drive fluid, and a high specific gravity torque converter fluid were supplied to prospective customers. Three phosphate esters were sent to Douglas at their request for additive solubility studies. III. REFERENCES 1. Final Report No. 620, "Hydraulic Fluids and Synthetic lubri cants", 117-2080 by R. E. Hatton, May 15, 1952. 2. Final Report No. 728, "Functional Fluids", 117-2380 by jR. E. Hatton, May 21, 1953* jM * *r> i *I * - > i ii 3. Final Report No. 936, "Functional Fluids - Application iResearch, 1952r54", 117-2506 R. E. Hatton, ,L. W. Bannister if&lO14.elc4^Auguat ;4,i 19644I I k. $4 ' ' ' ` it \ i E-felt llfcll lit' I I If I II !!? liillil DSW 620928 ] try vw rr # STLCOPCB4094956 44. Tentative Process P-553# "Blending of Pydraul 600", 117-2815 by R. E. Hatton, Sept. 24, 1954. : =' < f f: < ' ~ " 5. Tentative Process P-607, "Blending of Pydraul 150 (Fluid OS-57)", 117-2815 by R. E. Hatton, Kay 20, 1955. 6. Tentative Process P-628, "Bleeding of Fluid OS-67", 2-02 750.01-2815 by R. E. Hatton, August 18, 1955. 7. Final Report No. 1333, "Navy Shipboard Fluid - Process Development of OS-70, Part I", 2-02-750.01-3011 by R. S. Mitchell, November 11, 1955* IV. EXPERIMENTAL WORK AND DISCUSSION A. Pydraul F9 1. Vl3CQ3lty Index Improvers Pydraul F9, Monsanto's medium viscosity Industrial fire resistant hydraulic fluid and lubricant, consists of a base stock and additives, one of which is a viscosity index improver. Monsanto's Santodex was used for this purpose. It was decided for business reasons to suspend the manufacture of Santodex and it therefore became necessary to find a replacement. It appeared that Acryloid 794 was the least expensive purchasable replacement possible and its use In Pydraul F9 was studied. Solubility characteristics of Acryloid 794 were found to be similar to those of Santodex, being very miscible with Aroclor 1248 and essentially insoluble in tricresyl phosphate. However, it was quite readily soluble in Pydraul Base, the mixture of Aroclor 1248 and tricresyl phosphate -ormally used. Efforts to induce separation from the Base were unsuccessful. It was found that 2.5# Acryloid 794 in Pydraul Base gave about the same properties as 4.2# Putoiev. : series of fluids were prepared and their properties determJ.r.au. The data are as follows: Sample BD Viscosity,C3.210F. 6 *5.91 viscosity,cs.100F. 53*51 Viscosity Index + 34 ,Pour Point,F.i 1 , + 5; 6.02,t | 5.89 | >5.96 54.83 53.53 53.79 + -,5 5.83 * 53,82 ' DSW 620929 STLCOPCB4094957 I ,, , Samplea 1, A, B, C, and D were prepared from 45.0$6 JtriclreByl phosphate, 52.5# Aroclor 1248 and 2.5# Acrylold 794 using various lots of raw materials. The values obtained give some Indication of variation In property to be expected In normal formu lation. These samples met regular Pydraul F9 specifications for viscosity. The specific gravity was slightly greater than the 1.26 1.28 range normally allowed and sample 1 had a pour point higher than the specification value of C 'F. maximum. However, this was not considered serious and had previously been observed as a normal variation between batches. Sample E was prepared from the same tricresyl phosphate and Aroclor 1248 as sample D. Santodex was used in sample E and Acrylold 79^ in sample D. Thus these two samples give an exact comparison of changes resulting from change In viscosity index improver. The data thus far discussed indicated that Santodex could be replaced by Acrylold 794 in Pydraul F9. Therefore, a five gallon sample was prepared and sent ,to Douglas for evaluation and ___ comparison to Pydraul F9 in certain functional tests. The properties of this sample, called FH-103, are as follows: Viscosity, 210F. Viscosity, 100F. Viscosity Index Specific Gravity,25/25C. Acidity Pour Point Flash Point Fire Point 5.96 c.s. 54.6 c.s. -L 32 1.2694 0.03 NN 03F. 400F. 700F. The thermal stability of regular Pydraul FO was com pared to that of FH-103. Beakers of both fluids were placed In the oven and samples removed periodically. The oven temperature was 150C. throughout the test. Data ar. as follows: Time in Days rvC 1 d 1 ^ Pydraul F9 La FH-103 I | tt4f t1 .35, |42 0.20 C.48 0.78 1.46 3,6 11 i DSW 620930 _i STLCOPCB4094958 v. . r5 each Mterial^ *Thads observatloris indicate that the changed in vis cosity index improver from Santodex,to Acryloid 794 will have little effeot on thermal s- tability.. : : 4r-; ' f , ' : fi .: : i> Pump testing at Douglas showed that PH-103 was less shear stable than Pydraul P9 made from Santodex. It was felt that, if possible, a product of better shear characteristics should be found. A series of viscosity Index improvers were evaluated in Fydraul type formulations for shear stability. The Diesel Injector Shear Test was used. The test Involved passing the fluid through a Diesel injector five times and measuring viscosity before and after the test. The fluid was then again passed through the injector five more times giving a total of ten passes and viscosity again determined. Shear was measured in viscosity change. This test was carried out cn a series of samples and the data obtained are as follows: Sample Composition, wt. * Aroclor 1248 . Tricresyl phosphate VI Improver Santodex Acryloid 794 Acryloid 763 Acryloid 710 Acryloid HF855 Shear Data lginal viscosity 210F. V.I. 'ter 5 ;passes 210F. 100'F. V.I. loss In vise. at 100F. `ter' 10 passes - 210F. 100P. ; V.I ' iqsr [ BD 53.8 46.2 None 51.6 44.2 4.2 52.5 45.0 2.5 52.5 45.0 2.5 52.5 45.0 2.5 52.5 45 0 2.5 3.80 39.19 -258 S ,77 53.55 +22 5.99 54.96 +33 5.74 54.10 +17 5.67 54.13 +9 5.: 50.1 -24 39.21 -258 0 : .V 5.78 tfS h . ;8 42.59 -134 76* i1 *- 4.26 41.89 -159 83* 4.52 *t-. 67 4.< 44.58 46.17 47.: -120 -98 -77 64* . 53* 32* | M k 4.41, 4.54 4.77 >.38! .45.031 .46.25 DSW 620931 STLCOPCB4094959 The composition of the samples is listed In the table. One batch of Pydraulbase (Aroclor 1248, trlcresyl phosphate, sili cone defoamer) was used for all samples to eliminate variation In base stock viscosity. Hie data Indicate that Santodex and Acryloid 794 are comparable In shear with Acryloid 794 being slightly poorer. Shear stability Increased In order of Acryloids 794, 763, 710, and HF855. It should be noted that insufficient Acryloid HF855 was used In Sample F to give a fluid meeting Pydraul F9 specifications. Three weight percent should be sufficient. Probably slightly more shear would have been experienced at that viscosity index improver level than given in the table but certainly not much. Based upon these data and economic considerations, it was decided to use Acryloid 710. Five gallons of a Pydraul F9 formulation was 'ent to Douglas for pump tests. The material was labelled FH-105 and consistedof 52.5# Aroclor 1248, 45.0# tricresyl phosphate, 2.5# Acryloid 710 and 50 ppm. DC 200-350 cs. at 25C. In studying this formulation it was noted that the Acryloid 710 does not seem as potent as either Santodex or Acryloid 794 in that less viscosity index improvement is given for the aarne thickening (as indicated by 100F. viscosity). Specifications stated that Pydraul F9 should have a minimum viscosity index of 15 and a vis cosity at 100F. of about 240 SUS (52 c.s.). Fluid FH-105 was a compromise since it was desired to stay as close as possible to present Pydraul F9 properties. The properties of FH-105 are given in the following tabulation. Included are data on Pydraul F9 con taining 2.75# Acryloid 710 (A) and 3.00# Acryloid 710 (B) which Indicate the effects of increased concentration. Sample FH-105 B Viscosity,210F. Viscosity,100F. Viscosity Index Acidity Sp. Gr. 25/25C. Four Point Flash Point Fire Point 5.80 cs. 56.20 cs. + 11 0.05 NN 1.285 0'F. 395 F. 68oF. 6.05 cs. 5b.03 c s. t 24 1.28:- 6.28 cs. 59.94 cs. + 33 TX . C.W<-\Q 4_ + 5F. After testing by Douglas, a formulation change was approved and an amendment made to the manufacturing process for f M ! Pydraul F9 (amendment?dated June -2, 1955). Pydraul F9 produced I .after this date had the composition listed for FH-105 above. Speel' fications for Pydraul,. F9 were amended to Increase the specific gravity range ;to .be ifroni 1. !5 0 1.293. .Complete specifications : Uc ' Rydrat]|; F9 afidMic Ltd DSW 620932 STLCOPCB4094960 Moisture Acidity Pour Point Sp. Or. 25/25#C. Viscosity at 100P. Viscosity at 210F. Viscosity Index x 7 'i Cloudy-liquid, free of sedlbentf I 0.20#, maximum 0.15 NN, maximum 0P., maximum 1.275 to 1.295 45 to 6o cs. 5.2 to 6.1 cs. 5 minimum Thermal Stability The thermal stability of Pydraul F9 was studied at 150C. in conjunction with a series of tests on other fluids. The data are recorded under part C-4 of this section of the report. J. Lubricity Additives The Navy was faced with the problem of selecting a fire resistant hydraulic fluid for shipboard use. IXiring their evalua tions, it was found that Pydraul P9 did not perform as well as certain competitive triaryl phosphate fluids in a special bearing test. One approach to the problem Involved the use of additives which might be expected to reduce wear. A series of samples were prepared containing one percent of the following materials in Pydraul F9 and in a trlaryl phosphate (Cellulube 220): Santolube 393, RT-53A, RD 18-588, and Duomeen T Dioleate. These samples were labeled FH-108 for untreated Pydraul F9; PH-109,`FH-110, FH-111 and PH-112 represented the additive solutions in Pydraul F9 in the order listed above. Code numbers PH-113- WH-114, FH-115, FH-116,' and FH-117 represented the same series using Cellulube 220 as the base material. Douglas tested these materials and found that only Duomeen T Dioleate reduced wear in the Paxex Wear Test. This additive was only soluble at the cne perce..y level \ seating the mixture to about 6oC. *: In view of these results, an additive treated Pydraul F9 was submitted to the Navy for bearing test3. However, in this test, no advantage was found for the additive-treated Pydraul F9- It would appear tliat little correlation ^exists Jbgtweeru wear as*. i measured by the Falex machine and bearing* fatigue life* as measured ,.y the Navy test. I 4 u Hi tu DSW 620933 STLCOPCB4094961 *? ~ * y * e S. J. : ' 4. Other Trloreayl Phosphates f; An appreciable savings In the cost of Pydraul F9 would result if gasoline grSdb trlcresyl phosphate (0 grade TCP) could be used in the formulation Instead of plasticizer grade trlcresyl phosphate. Using the established formulation, a Pydraul type sam ple was prepared from 0 grade TCP made from Shell cresyllc acid 2000AA. A control batch was also prepared from regular A grade trlcresyl phosphate using the same lots of additives used to pre pare the evaluation sample. The analyses of these batches, as well as of the trlcresyl phosphate base stocks are as follows: Pydraul, Pydraul, Trlcresyl phos- TCP, G grade Control Evaluation phate,A grade from 2000AA BatchBatch (for control) (for evaluation) Viscosity,cs. + 210F. + 100F. Pour Point 5.99 54.6 0F. ' 6.45 68.5 +10F. 4.26 52.4 - 20 F. 4.84 45.9 -10F. The differences In viscosity between the two batches would not rule out the use of this phosphate ester. However, the high pour point of the formulation using G grade TCP would be too high to be satisfactory. Using the established formulation, the G grade TCP is not satisfactory for use in Pydraul F9. Another sample of G grade TCP was examined. This material wa3 made from Productol cresyllc acid in Dept. 50 of the J.F. Queeny plant. Data are as follows: Viscosity, cs. ' + 210F. + 1C0F. . . 59.74 Viscosity Index + 19 ' Sp. Gr. 25/25C. - ? i * - j k f ; ! f | 1 *' 1.1559 .: ' t* f t< r5 DSW 620934 STLCOPCB4094962 Ml] 1. Formulation Studie1s* . s. ri- '' i " " 4 Pydraul F9 oanbeolassed as a medium viscosity hydrau lic fluid, its viscosity at 100F. being 250-275 Saybolt Universal Seconds (SUS). Although Pydraul F9 had found wide usage In a variety of hydraulic systems, it appeared that certain pumps require 600 to 900 SUS fluids. ITie Sales Department indicated that a real need exists for Pydraul-type fluids having these viscosity proper ties. Some interest had also been expressed in a 150 SUS Pydraul- type fluid. Laboratory work was undertaken to formulate fluids from Aroclor-tricresyl phosphate base stocks. Satisfactory fluids having 100F. viscosities of 900, 600, and 150 SUS were developed. All these fluids are derived from the same chemical type compounds as Pydraul F9, all being based on tricresyl phosphate and Aroclor mixtures. Therefore, it is felt that these fluids would be very similar to Pydraul F9 in stability, flammability, and general utility. Two general types of base stocks were studied for each viscosity desired, one consisting of a 50:50 blend of tricresyl phosphate and an Aroclor and the other consisting of a 25:75 blend. The composition and the properties of the selected formulations are given in the following table. Fluids A and B are in the 600 SUS class, C and D are in the 900 SUS class, and E and F are in the 150 SUS class. Fluids B, C, and F are the fluids of choice based upon property and economic considerations. Fluid Designation Code Number Composition,weight $ Tricresyl phosphate Aroclor 1242 Aroclor 1248 Aroclor 1254 Aroclor 1200 Acrylold 794 Properties - Viscosity,100 F,SUS cs Viscosity,210F,SUS *' ' C8.. Viscosity Index Pour Point, F. i. So.IG 3%Pl * 0 ?! ABc D HV-5.5 HV-1-4 HV-2-4 HV-3-2 47.25 24.0 24.5 47.25 36.0 36.0 4.0 a;-. 4.0 2.0 609 630 151 136 65.4. | 59.0 1 11.8* * *9.9 * +83 +33 +15 ,/ ft +15 1*.220| 924 195 65.8, nR EF HV-7-2 HV-6-2 49.0 49.0 24.5 73-5 2.0 2.0 2271 DSW 620935 STLCOPCB4094963 -.Jp ' Silicons defoamer was added to each fluid at a concen tration of fifty parts per million. Viscosity at 50P. was found to be 2250 cs. for fluid A and 4025 cs. for fluid B. Cloud point for fluid A was +40F. Fluid B did not cloud to its pour point. It was decided that Fluid B would be developed as Pydraul 600. A Tentative Process (Ifc:j>ort No. P-628, August 18,1955) was written. A one thousand gallon batch, was prepared in the Interim Production Facilities. Properties of this material are as follows: Viscosity, 210F. Viscosity, 100F. Viscosity Index Specific Gravity,25/25C. Pour Point Moisture 9.67 cs. 135.8 cs. +26 1.364 +15F. O.Olg The product was sent to several prospective customers for evaluation. During the development of the fluids described in this section, a series of fprmulations were prepared and studied. Data for these formulations are as follows: Fluid Composition, $ by weight Desig- Aroclor nation TCP 1242 124b 1254 1255 # Viscosity 2l06F fF. Vis. PP cs. ~STJS cs. 8US Index F. HV Base HV-3 HV-4 HV-5 HV-6 HV-13ase 25 HV-1-4 24 HI'- 1-6 23.5 HV-2- Base 50 HV-2-3 48.5 HV-2-4 48 HV-2-6147 I 37.5 37.5 36 36 35.25 35.25 4.84 42.1 71.1 330 - dS>2 +10 3 8.07 52.7 99.5 461 + 24 4 C 9.44 1 Kj . ^`Aj 57.4 111.1 62.4 122.8 515 + 569 + 55 74 6 12.50 63.4 136.3 631 + 89 4, t.'i 40 71 . 1 4 9. >'l - n _ -0~ - 6 13.53 72.5 174.9 810 PJ>5 i 20 33 +15 74 6.04 46.0 131.8 611 - 309 +10 3 9.91 59.0 175.2 812 - 21 4 11.81 65.8 199.4 924 +, 17 +20 6 15.69 - 80.7 234.3 5. -*4 43.6 145.9 676 - 620 +25 ,8,r j>5 53.. 7 194.2; 900 L153 i+2S 53. 6ci5i224. ;1040 If DSW 620936 STLCOPCB4094964 II Fluid iComposition, %by yelght Deslg- A__ro__c_l_o_r nation TCP T42 124ET 1254 T250' * Vl3Coslltt;y WFT cs. ~5US cs. Vis. PP HV-4- Base 25 HV-4-3 24.25 HV-4-6 23-5 HV-5- Base 2?. 25 HV-5-3 HV-5-6 23.5 HV-6- Base 25 75 HV-6-2 24.5 73.5 HV-6-3 24.25 72.75 HV-6-6 23.5 70.5 HV-7- Base 50 50 HV-7-2 49 49 HV-7-3 48.5 48.5 HV-7-6 47 47 hv-8- Base 42.1 HV-8-3 40 HV-8-5 4o 37.5 37.5 36.38 36.38 3 35.25 35.25 6 6.60 47.8 298.5 1390 - 814 +35 12.41 68.0 419.8 1945 - I60 20.88 102.3 573 2650 + 7 +30 75 72.75 70.5 8.43 53.9 713 3300 -1165 +4o 15.83 81.2 900 4170 - 288 25.16 121.0 1082 5020 - 51 +35 2.80 4.41 5.39 8.84 35.6 40.7 43.9 55.3 21.2 32.8 37.5 59.4 103 - 208 - 5 154 - 5 -10 175 + 79 276 +133-5 57-9 55 55 3.28 4.67 5.44 8.53 37.2 41.6 44.1 54.3 25-6 34.1 36.9 53.7 122 - 153 -lcT 159 + 25 -10 172 + 87 249 +131-5 4.99 8.75 12.14 42.6 88.8 55-0 130.6 67.0 166 412 - 372 +15 605 - 4 769 + 57 +15 * Acrylold 794 In order to make the Pydraul serias consistent and to prevent the stocking of a large number of Acr-ylolds, it was decided to change from Acrylold 794 to Acrylold 710 in Pydraul 600. A sample of Pydraul 600 from Acrylold 710 (FH-107) was prepared -.rd sent to Douglas for evaluation. Properties are- follows: Sample FH-107 Viscosity, 210F. Viscosity, 100F., Viscosity Index . L Acidity f I" S If Sp. Gr. 25/25rC. Pour Point ; { I ' 9.24 cs. 134.5 cs. +11 , 0.06 NN 1.352 T C T7 , ;4150K DSW 620937 STLCOPCB4094965 ^ / 4.-"' -JM _ ^ lition of?!P^107"l8ras follows _________ 1248, 36# Aroclor 1254, 24 tricrssyl phosphate, 4 Acrylold 710 and 50 ppm DC 200-350 os. at 25 *C. An amendment was made to the Tentative Process on Sept. 12, 1955 end Pydraul 600 made after ? that date had the same composition as FH-107. 2. Viscosity Data Viscosity data over a ide temperature range were determined for Pydraul 600 and are as follows: Viscosity, 210 F. 130F. 100F. 50 F. cs. 9.83 46.0 135 3910 3. Solubility of Water In Pydraul 600 The solubility of water In various fluids was deter mined at room temperature and at 210F. The procedure for the determinations at room tempera ture was as follows:. A sample of the fluid was stirred from 1-1/2 to 2 hours with an equal volume of water by bubbling an air stream through the mixture to Insure intimate contact. The layers were_ allowed to separate about an hour. The ester layer was then centri fuged for 30 minutes to free it from occluded water. Samples of the ester were weighed in duplicate into tared stoppered flasks containing a mixture of benzene and methanol blanked with Karl Fischer reagent. The samples were then titrated with Karl Fischer reagent. ? The procedure for the determinations at 210F. was as follows: A sample of the fluid was a.irred for 1-1/2 to 2 hours with a large maintained excess of water by bubbling an air stream through the mixture contained in a la'-ge tube placed in a 210F. constant temperature bath. The layers were the' c.lTowed to separate for about 4 hours. The e.s* i-r layer v;ac .'e v, s:iov.ing no occluded water to be present In it. Using a warmed pipette, samples of the ester layer were weighed in duplicate into tared stoppered flasks containing a mixture of benzene and methanol blanked with Karl Fischer reagent. The samples were then titrated with Karl Fischer reagent. Hie results are listed.in the following table: i {* I l fI s if f Pydraul 150 OS-63 Pydraul 600 Soliibilitj ?oom. ; pill* ( 0.26*, f DSW 620938 STLCOPCB4094966 C m.hjr- - ;.y, *V-^W " ' 4 " i . :% Formulation Studies !' '' i : 1 - Many applications require the use of fire resistant hydraulic fluids possessing better low temperature properties than Pydraul F9. To,fill such needs, OS-57 was developed. Details of the formulation 'study axe reported in Pinal Report No. 988, "Func tional Fluids - Application Research, 1952-54", Job No. 117-2508. A Tentative Process (Report No. P-607, May 20, 1955) was written .under this job number and the name of the fluid changed to Pydraul 150 In order to make the Pydraul series consistent, it was decided to change from Acryloid 7'9^4 to AAecrryy]loid 710 in P_ydraul 150. A sample of Pydraul 150 from Acryloid 710 (labeled FH-106) was prepared and submitted to Douglas for evaluation, Properties of the sample are as follows: Sample FH-106 Viscosity, 210F. Viscosity, 100F. Viscosity Index Acidity Sp. Gr. 25/25C. Pour Point Flash Point Fire Point 7.55 c. 31.06 c. +169 0.07 NN 1.125 -55F. 390F. 470F. t Theicomposition of FH-106 is as follows: 6956 2-ethyl- hexyl diphenyl phosphate, 23^ Aroclor 1242, Acryloid 710 and 50 ppm DC 200-350 cs. at 25C. It was necessary to use 8^ Acryloid 710 to obtain the desired properties ror Pydraul 150 as compared to the 7.5% Acryloid 794 previously used. An amendment was made to the Tentative Process on Sept. 12, 1955 and Pydraul 150 subse quently produced was formulated by this proceci- - 5 i ' f 2. Viscosity Data -- #; *i Viscosities over a wide temperature range were deter- mined for a samplelof Pydraul 150 and are as follows: i - it Vis^slty; cs/ *f J f I if- k-i l t DSW 620939 STLCOPCB4094967 <p* II' iml %1 Hw 3. Solubility^of Water In Pydraul 150 . i t . r. v I . < I The solubility of water In Pydraul 150 was found to ; > . < be 0.50# at room temperature and 1.2# at 210#F. Details of these ?'** determinations are given under section B-3 of this report. 1 4. Thermal Stability Previous work on the thermal stability of Pydraul 150 was conducted at 125C. or above. It was felt that such studies should be extended to temperatures in the range of 110C. and comparative data for fluids such as Skydrol 7000, Skydrol 500, and OS-54 should be collected. Even this temperature is somewhat above normal operating temperatures in hydraulic systems. The method used was as follows: One hundred gram samples of the fluid were placed in beakers and the beakers placed in an electrically heated oven at 110C. After the desired time had elapsed the samples were removed and examined. The data for this series are as follows: Time in Days 0 Pydraul 150 37 14 21 28 35 42 49 56 63 Acidity,NN Viscosity, cs.,210F. 100F. Skydrol 500 0.08 O.36 0.6l 1.1] 1.66 2.96 3.9 8.3 11.7 7.73 7-58 7.58 7.79 8.06 30.45 29.99 30.27 30.96 31.09 Acidity,NN 0.03 0.11 1.21 5.7 Viscosity, cs.,210P. 4.02 4.11 100F. 11.94 12.44 1118.2 27.8 28.7 40.9 43.1 53.7 4.45 13.41 4.96 16.26 Skydrol 7000 i> if Aciaity,NN 0.-13 0.87 1.75 4.4 Viscosity, cs., 210F. 4.05 4.10 t j t =. 100F. 15.90 | 5 *16.3.5 * Fluid OS-54 7 .0 11.6 16.9 29-2 43-7 4.22 4.51 17.26 : i 19.00 : * * ? 138 152 , \ f. | t- ' I 1.0420 i too Im DSW 620940 STLCOPCB4094968 :* rtfeighfc 'lolsei *fter?63 days^ were *aS>out 12J6 or Pydraul" |150*l 23# for Skydrol 500, 21# for Skydrol 7000,. and ll for Fluid OS-54. Skydrol 7000 separated Into two layers After 49 days. All fields darkened on heating,the amount of darkening being greater with greater acidity development. Considerable differences In thermal stability may be noted. Fluids OS-54 and Pydraul 150 are more stable to heat chan either Skydrol. All fluids appear to decompose In the normal manner for alkyl aryl phosphates, liberating a volatile material and developing acidity. These data together with previous data can be used to determine safe maximum temperature-time operating limits. For ' comparative purposes, the time required to develop 1.0 NN acidity may be used. At 110C. these times would be about 3 days for Sky drol 7000, 6 days for Skydrol 500, 12 days for Pydraul 150 and 25 days for Fluid OS-54. Similar times for Pydraul 150 are about 4 days at 125C., one day at 150C. and about 6 hours at 175'C., illustrating the time-temperature relationship. Similar data were obtained for Pydraul F9 at 150C, as follows: > in Days Acidity, NN Viscosity, C3. 2lOdP. lOtrF 0 0.17 5.62 45.08 3 0.27 7 0.33 5.24 47-72 14 0.82 21 2.81 5.23 48.22 28 4.1 35 7. *c - t yw 52.62 49 18.9 56 37.4 63 48.1 * The weight loss was about 30$ Vr; C? days. These data demonstrate the increased thermal stability of the Pydraul F9 fluid containing tflcresyl phosphate as compared to those reported above which contain alkyl aryl phosphates. fluid fires, the invyoc lved.and 5 a 9 DSW 620941 STLCOPCB4094969 1. 03-54 OS-54 was originally developed as a fire resistant power steering fluid and became of interest to the Navy. Details are recorded in Pinal Report 988, Job number 117-2508. Hie thermal stability of OS-54 was Btudled and detailed data are given under section C-4 of this report. 2. OS-6? After a thorough examination of all shipboard hydraulic systems, the Navy had concluded that the low temperature properties of Pydraul F9 were not completely satisfactory. Pydraul F9 had previously passed flammability, pump, and bearing tests. A fluid somewhat similar to Pydraul F9 was selected from our back-log of formulations and a rust inhibitor added. Such a material, called Fluid OS-6?, should meet the low temperature and the antirust requirements of the Navy. A one pound sample (A) was prepared and submitted for evaluation. Properties were as follows: . Sample ` AB Vl3cosity,cs.,210F. 100F. 20 F. Viscosity Index Sp. Gr. 25/25C. Flash Point, F. Fire Point, F. Pour Point, F. Acidity, NN 5.41 37.4 3560 82 1.246 360 660 -10 -- 5.46 37.0 84 1.246 ?85 650 -10 0.11 Fluid OS-6? consisted of 48.4$ tricresyl phosphate, 48.4$ Aroclor 1242, 5.0$ Acryloid 794, 02$ Sartolube 70 and 50 ppm DC 200-550 cs. Satisfactory results obtained in preliminary tests led to a request for more fluid and several gallons (Sample B) were prepared. * s . i | The solubility of water in OS-63.was found to bej,0.24$,. at room temperature and 0.62$ at 210F. Details of the *determina-' tion are given in section B-3 of this report'. ' i |,il ,1 t i-U i DSW 620942 mi STLCOPCB4094970 , ~ i" ' vi v \' tilvk'W . r ^ 4 v. ^ ? sf- $ .16 P 1 I OS-66 i IP The Navy requested a Pydraul 600 type fluid possessing improved shear characteristics. Accordingly, a gallon of Fluid OS-66, which was Pydraul 600 containing Acryloid HF655M, was pre pared. The properties of this batch were as follows: Viscosity,cs., 210F. Viscosity,cs., 100F. Viscosity Index Acidity Sp. Gr. 25/25C. 9.24 128.8 +20 0.05 NN 1.3596 This material was sent to the Navy under Lot Number Y-2175. 4. 0S-70 (Trlaryl Phosphates) The Navy's evaluation of many fire resistant fluids -- led to the adoption of Cellulube 220 because of Its performance In a special bearing test. Cellulube 220 Is a triaryl phosphate fluid produced by `the Celanese Corporation of America. In order to participate In sale of fluid to the Navy, two approaches were taken. The first approach involved the examination of Pydraul F9 failure In the particular bearing test as contrasted to satisfactory operation In the field for many years. (See Section A-3.) The second approach concerned the preparation of a product equivalent to Cellulube 220. Studies along this line were started under this Job number. However, the major portion of the work was done under Job number 2-02-750.01-3011 and all data will be reported under the latter Job number. E. Pydraul AC (OS-67) A need existed for a fire resistant air compressor lubri cant. Work was started between Mr. Ho re ton c- ~-;.u3las ana Standard Oil of California persormei to develop ... fire resistant air com pressor lubricant. Fluid OS-67 which consists of 43# tricresyl phosphate and 57# Aroclor 1254 resulted.* *-- ------------- ` ' ----------------------------------------- -- ' ~. A. - WsXa--mple was prepared^ InXii our laboratory and physical properties were determined and compared with the Douglas sample (LHD''). ~Da'ta are as follows: . !f Sample* i f f ' f ` I I * h # OS-67 t LHD Viscosity, iosityj wti ; in: DSW 620943 STLCOPCB4094971 Cation ^expected nor Latlons in raw material. 9:A - Larger quantities 4were needed for development work and a tentative process (Report No. P-628, August 18, 1956) was written. Satisfactory large scale tests resulted In the wide spread adoption of OS-67. Its name was changed to Pydraul AC. P. Steam Turbine Fluids A steam turbine fire resistant lubricant was developed under Job number 117-2508. Four gallons of this fluid., OS-58-1, were prepared for submission to prospective customers. Its pro perties were as follows: Viscosity at 210F. Viscosity at 100F. Sp. Gr. 25/25C. Pour Point Acidity 5.43 cs. 39.5 cs. 1.304 -5F. 0.05 NN This further quantity was required because of promising results in preliminary studies'. The solubility of water in OS-58-1 was found to be 0.12$ at room temperature and 0.39$ at 210F. Details of this determina tion may be found in Section B-3 of this report. Work on steam turbine fire resistant lubricants was con tinued under job number 2-02-750.01-2949. G. L-3A Fluid A sample of used Fluid L-3A from Axelaon Manufacturing Co. was examined. This material had been used 200 hours in their Alternator Drive unit at l80F. to 2l0oT. Problems concerning improved lubricity with decreased traction proper"through possible contamination had beer, experience-.-,. . The properties of the sample as compared to those of the fluid originally sent are as follows: t ..Sample p ; *.4 f * " f <! * Viscosity,cs., 2101F. Used 3.24 M iNewt ti iIlsctoselty Inrdexj ii DSW 620944 STLCOPCB4094972 vjmm-m- mrynw m* > J? ft*+ % jS sample of used fluid was quite cloudy and normal filtra tion techniqueawould not produce a clear material. h Hie acidity of the used fluid seemed abnormally high. Changes in other properties indicate possible contamination. A reserve sample of new fluid was sent to Douglas who plan to run comparative lubricity tests. Larger quantities of fluid were desired by AxelBon for further test work and 20 gallons were prepared. The properties of this were as follows: Viscosity, 210P. Viscosity, 100F. Viscosity Index Acidity Sp. Or. 25/25C. 3.91 C3. 15.02 cs. + 76 0.38 NN 1.062 L-3A fluid consists of 60# tricresyl phosphate and 40# Ucon DLB 50-E. It has also been known as OS-22. H. OS-41 The Ford Motor Company expressed interest in OS-41, a proposed synthetic high specific gravity torque converter fluid. Three gallons were prepared and submitted for tests. The material met specifications in all respects. OS-41 consists of 48# 2-ethylhexyl diphenyl phosphate, 48# Aroclor 1248, 4# Acryloid HF855 and 50 ppm DC 200-350 cs. at 25C. I. Phosphate Esters for Douglas Douglas requested samples of a l"- molecular weight di alkyl aryl phosphate and a high molecular weight alkyl diaryl phosphate for test work concerning additive solubilities. Samples of n-decyl diphenyl p.hosphate and 2-butyIoctyl dic-.r^oyi phosphate were taken from reserve supplies and sent to FH-1Z2 and FH-123, respectively. Dimethyl phenyl phosphate was prepared and puonutted to Douglas as FH-121. Details of preparation are as follows: . In general accordance with U.S. Patent 2,426,691, dimethyl phosphoryl phloride |was prepared;as follows: Phosphorus trichloride (262 ml., 3'moles)was added dropwise to a cooled solution of 372 ml. (9-2 moles) of methanol and 500 ml. of benzene, the addition re quiring v2.hoursi at ^-12C. j. During* the, nex>. hour, while^the .reaction arsed :-nat Vcfcut &wa 4^1 Id! 2201 111 DSW 620945 A\ STLCOPCB4094973 V%* %I-ff 7i \1 5t Then ohlorlne gas was bubblsd ixff&tf -2 to +12*C. (140-220 n*n.) ' until the reaction mixture turned*yellow and the temperature began to fall; 3.5 hours were required;'for the chlorination and the chlorine uptake was 213*5 g Just 0.8 g. over the theoretical. The cooling bath was then lowered and the pressure In the system was reduced to 50 mm. where It was held as the reaction product wanned to room temperature during the next three hours. The crude dimethyl phosphoryl chloride was added dropwise with stirring at 0-5C. to a sodium phenate solution, which had been prepared from 252 g. (3*15 moles) of plant lye, 420 ml. of water, and 296.4 g. (3.15 moles) of phenol. The addition required 5 hours, after which the reaction mixture was stirred for 4 hours without cooling. luring the latter period, the alkalinity of the mixture was maintained by additions of lye as needed. Layers were separated, and the organic layer was washed with two 900-ml. portions of 2$ lye solution, three 900-ml. portions of 1$ lye solution, and four 1000-ml. portions of water. The last two water washes were treated with a few drops of sulfuric acid to get them to separate. After washing, the product was dehydrated under vacuum until-essentially all benzene had been removed. At this point 50 ml. of water was added and the dehydration was finished at full water pump vacuum to 110C. The dry ester was stirred with 3 g. of Nuchar C-145-N as it cooled, then was filtered through Attapulgus earth. The finished dimethyl phenyl phosphate had the following properties: n 1.4862, sp. gr. 25/25C. 1.2262, NN 0.30, and APHA 300. The yield wa3 322 g. (55.1$). V. CONCLUSIONS A new viscosity index improver wa3 accepted for use in Pydraul F9. The substitution was necessary uecuucc* of the end of manufac ture of Santodex. Acryloid 710 was chosen because of resistance to shear, ability to produce a satisfactory Pydraul F9, and economic considerations. Acryloid 794 was rejected bo, :u1= of poor shear stability. Amendment was trr.de to the M;'ufac lurL..g Process for this formulation change. It was shown that gasoline grade tricresyl phosphate cannot be used as a direct replacement for, plasticizer grade in Pydraul F9. A high4 viscosity7 fire resistant 'incirslrial-hydraulic fluid? ' * was developed and introduced to the market as Pydraul 600. Various properties, were determined to assist iri Its utilization.. A Tenta 'tiv" eS f,-Erodes" s ` Ik L DSW 620946 mm STLCOPCB4094974 hi TOP lamPydraulw150 temperature, low viscosity fire resistant Industrial hydraulic fluid, had previously been proposed for certain applications, further fomulatlon studies were carried out and a Tentative Process' Written.' ` Thermal stability tests Indicated that Pydraul 150 was similar-to Skydrol 7000 In resistance to thermal breakdown. The rate of -breakdown was shown to be dependent upon composition and temperature (Pydraul 150, OS-54, Skydrol 500, . Skydrol 7000, and Pydraul F9 were run 1r this series of tests). The data obtained assist in determining safe maximum operating temperature-time limits. Various physical properties were deter mined for Pydraul 150. The solubility of water in Pydraul 150, Pydraul 600, OS-58-I, and OS-63 was determined at room temperature and at 210F. These data are of particular value in the design of recovery systems for wet fluids. IXiring the Navy's evaluation program of fire resistant ship board hydraulic fluids, two distinct plans were followed by Monsanto. The first plan involved emphasis on Pydraul type fluids. A number of fluids such as OS-51*, OS-63, and OS-66 were submitted for evaluation. An additive was found through cooperative testing with Douglas that reduced the wear characteristics of Pydraul F9 in the Falex Wear Test. However, such improvement did not carry over to bearing fatigue life as measured by the Navy bearing test. The second plan involved the development of a triaryl phosphate fluid similar to an approved material (Cellulube 220). This pro gram was started and further work done under job number 3011. A fire resistant air compressor lubricant, Pydraul AC (OS-67) was developed by Douglas. Considerable promise was shown in large scale tests. A Tentative Process was prepared. Further samples of a proposed fire res'* rvt-arvc steam turbine lubricant, 0S-5&-1, were prepared for evaluation by Interested groups. Preliminary results were quite promising and the work was continued under Job number 2949. Samples of used L-3A fluid were examined. Contamination was suspected and found. Larger quantities of L-3A were prepared and supplied for further test work in an adhesion drive. * * Three gallons of OS-41 were prepared and submitted to Ford Motor Co. |f^r;^ti|l^ aji^ torque converter fluid, t - t * n-Decyltdiphenyl phosphate, 2-butyloctyl dicr^sy] phosphate, i i tar.d ^dlnrethy^iJ^eriyl .phosphate wer*e submitted va Douglas for , test o iWnffli DSW 620947 STLCOPCB4094975 fek VI. APPENDIX . .. .. . \ ySS_ . '. __ . ..... wm% ' "" ' "* ; ' ,. , .,, During the period- of this work, other studies in the field of functional fluids were in progress. A listing of Job numbers is as follows: '1 2813 - Skydrol 500 Investigations ;if -s ' - i- 2814 - Preliminary Screening Evaluations - Functional Fluids 2816 - Silicate Ester Fluid Investigations 2919 - Application Research on Silicate Ester Fluids 2921 - Exploratory Research on Functional Fluids - 1955,56 2922 - Minor Plant Investigations and Consultations on Functional Fluids - 1955,56 2949 - Synthetic Steam Turbine Lubricants 3011 - Navy Shipboard Fluid 3012 - High Temperature Fluids llfall i. ' Notebook page numbers are as follows: -L.W.B.: A-66915, 16 -i R.S.M.: A-54559, 62, 72, 74 A-59342, 44, 46, 49, 50 A-60191 A-63426, 40 , A-67454, 58, 74, 500 R.S.H./A.J.B.: A-52233,436, 37, 38, 4Q, 41, 42,^43, 48, 49 , ,, , .f 'A-65051J52,'53? 54 , 62, 0,167, *68; ?70, 71/ 72, 73, 74-, *75.- M ? 77, 78, 79, 80 | - *T fe.il i/ii ^ DSW 620948 STLCOPCB4094976