Document wq7jYKd4wq59zZ5gQLQDY4NvD

: i STLCOPCB4073614 > PROTECTIVE COATiliGS - A LASSE . GROWING IMPORTANCE OF SYNTHETIC RESINS IN COATINGS Pictures and inscriptions painted on Egyptian tombs and Chinese temples as long ago as 2000 B.C. mark the earliest known use of paint-like materials. Paint technology has still not changed its predominant reliance on naturally occurring materials, symbolized by pails of white lead and linseed oil. True, modernization has seen the development of new pigments, better vehicles, and more efficient manufacturing techniques, but the old stand-bys are still in use. - The development of synthetic resins, however, has freed industry from dependence on natural resins and has enabled the production of faster-drying and more-durable and more-resistant protective coalings than could be made from natural raw materials alone. The nitrocellulose- lacquer development in the early 1920's revolutionized automobile finishing. The discovery of alkyd resins in the late 1920's and the introduction of latex paints in the late 1940's further broadened the outlets for protective coatings and increased the sales of these products. Now, annual sales of protective-coatings materials amount to more than 600-million gallons, valued at more than 1.5-billion dollars. ROLE OF PLASTICIZERS IN PROTECTIVE COATINGS Success of the new synthetic resins in protective coatings often depends largely on the modi fiers used with them. Plasticizers--one of the most important types of modifiers--can im prove such vital characteristics as flow, levelling, brushability, impact resistance, drawability, gloss, and luster. As a basic producer of more than 80 different plasticizers, Monsanto Chemical Company is an important partner with synthetic-resins manufacturers and protective-coatings producers in the selection and development of the particular plasticizer system that imparts the best all-around durability, performance, and economy for every coating application. This bulletin is presented to help protective-coatings manufacturers formulate better finishes. It should be remembered that each suggested starting formulation should be carefully evaluated by the formulator in both laboratory and service tests before any final formulation is based on information contained in this bulletin. Of course, Monsanto's technical-service representatives are prepared to offer unbiased recommendations for plasticizer systems to meet any perform . ance requirement, without obligation. \ DSW 321965 STLCOPCB4073615 CONTENTS MONSANTO PLASTICIZERS IN CELLULOSIC COATINGS ........................... I Nitrocellulose................................................. * Ethyl Cellulose ........................................................................................................ 7 Cellulose Acetate-Butyrate................................. ................................................... Cellulose Acetate.............................................................................. IS MONSANTO PLASTICIZERS IN VINYL COATINGS.......................... 17 Poly (vinyl Acetate) ............................. *....................................................... ........ 17 Poly(vinyl Chloride) ............................................................................. 23 MONSANTO PLASTICIZERS IN RUBBER COATINGS ....................................30 Chlorinated Rubber ........ SO Chlorinated Polypropylene ........................................................... 36 Styrene-Butadiene Copolymers ...................................................... 37 Synthetic Rubber ................ 40 MONSANTO PLASTICIZERS IN OTHER RESIN COATINGS............................41 Epoxies ............... --41 Acrylics ................................................................................................................... 45 Polyamides............................................................................................ --................46 Zein ..........................................................................................................................46 Varnishes and Alkyds..................................................... 49 Silicones ................................................................................................................... 49 Phenolics ................................................ ..........................'..................................... 50 Melamine ...............................................................................................................--50 Shellac ......................................................................................................................50 OTHER MONSANTO PRODUCTS IN PROTECTIVE COATINGS................... 51 Resin Additives ........................................................................................................51 Coating Modifier......................................................................................................51 Antioxidants ......................................... 51 Catalyst / Clarifier..................................................................................................51 Odor-Masking Agents ................................................................................. .*.......... 52 Preservatives ....................................................... ................................................... 52 Flatting and Thickening Agents ............................................................................52 MONSANTO TECHNICAL SERVICE.......................... 52 SHIPPING ........ ,................... ....................................................................................... 52 TECHNICAL LITERATURE .................... 54 "Rothkifcontalnod hirln h tot* censtrv*4 mrtcommendition to uit iry product Inccnttict with *N)h$ANTO#A*lShO WARSAKIItS AS TOTH ftT'.TSS OS VIRCHA.IMBIIMY OF AHY PRODUCTS RlFlRKtD TO, no |uir>fltt of utulKiory multi tiom idtjrKt upon con< RitMdtAlMBUtiCfltr ifC4*tunrH}ti9ni,in4 CiacUitnj ah liability tot any raiuitrtfioii w danuja," I DSV^ 321966 ) STLCOPCB4073616 . . jrtRk . ; ' f ' t 9 > MONSANTO PLASTICIZERS IN CELLULOSIC COATINGS NITROCELLULOSE . Nitrocellulose is the basic film former for lacquers. Both the R. S. (regular-soluble) and the S.S. (spirit-soluble) grades are generally used in lacquers. Films applied by these lacquers pos sess the following characteristics: ' . ' Fast drying Clarity Color stability Hardness Flexibility Mar and scuff resistance These lacquers are used for. a wide variety of coatings, including the following typical appli-. cations: Wood and furniture lacquers Plastics lacquers . Paper coatings and impregnants Metal lacquers Automobile lacquers ' Textile coatings . Aerosol lacquers Bronzing lacquers Nitrocellulose films, however, are quite brittle without plasticization. A wide variety of plas ticizers is used to improve the gloss, flexibility, and adhesion of these films; and the use of plasticizers increases the solids content of nitrocellulose films. The performance of various Monsanto plasticizers in nitrocellulose is shown in Table I. TABLE I--PERFORMANCE OF MONSANTO PLASTICIZERS IN NITROCELLULOSE FILM Flasticiier (SO FHR) Flexibility (Schopp.r Fold Cycl.t) Tensile Strength (P'J Elongation 1%) Control (none) Dibutyl Pkthalate Santicizer* 160 Triphenyl Phosphate Tricresyl Phosphate Santicizer 1-H Santicizer S . 20 10 14 24 -- 10 16 6660 2740 2610 4460 1220 2210 2210 . 6 4 10 6 24 7 11 ) Relative to permeability of unplasticixed film as 100%. Samticiur: Mottunfa) Chemical Company Ttadrmark. Rcfiiitrtd in U.S. Patent Office. Moisture Permeability m 100 65 19 56 28 41 62 STLCOPCB4073617 The use of nitrocellulose lacquers on furniture has assumed large proportions. These lacquers give excellent protective coatings. Shown below are several examples of wood-finishing lac quers: N, Ingredients R.S. Nitrocellulose (*/i-sec.)J R.S. Nitrocellulose (1/i-sec.)`I ^ R.S. Nitrocellulose (5-6 sec.) Maleic Resin (SS'yh in toluene) Non-Oiiduing Alkyd (60% n.v.) Santolite* MHP Santicizer. 160 or Dibutyl Phthalate Santicizer 165 or Dioctyl Phthalate Zinc Stearate Paste Castor Oil Hi-Flash Naphtha Toluene Xylene Ethanol Isopropanol Butanol Ethyl Acetate Butyl Acetate Crllosolve** Acetate Methyl Ethyl Ketone . . a) Maleic resin-based wood sanding sealer 1* _ 60 50 510 --__ IS -- 120* 18 210 105 17 18 -- 55 200 525 --- . Paris by Walghl 100 __ 70 60 IS __ 50 __ . -135 ' __ -- 55 60 no \-- 190 ' i* 100 -- -- 40 30 30 -- 17 -- 15 155 70 __ 15 65 __ __ __ 150 -- b) Clear, high-gloss furniture lacquer with good polishing properties e) Clear brushing lacquer d) 75-per cent nonvolatile in ethanol e) Zinc Stearate Paste composition: Ingredients R.S. Nitrocellulose (5-6 sec.) Zinc Stearate Magnesium Carbonate Castor Oil Hi-Flash Naphtha Ethanol Ethyl Acetate Butyl Acetate Parts by Weight 25 50 i 8.5 ' 90 58 45 17 * Saniolits: Monsanto Chemical Company trademark. Registered in U.S. Patent Office. 11 Tradematk of Union Carbide Cotp. 2 OS'N 68 STLCOPCB4073618 Another broad, area of application for nitrocellulose lacquers is in automobile finishing. Shown below are suggested formulations for the three coats used in the build-up of an automobile finish: Ingredients 4 Nitrocellulose (t/i-sec.)^ Nitrocellulose (Vi-sec.) Non-Drying Coconut Alkyd Blown Soya Oil ^ * Santiciier 160 or Dibutyl Phthalate Dioctyl Phthalate Tricrcsyl Phosphate Magnesium Silicate Fibrous Magnesium Silicate Dispersing if Grinding Agent . Zinc Chromate Red Iron Oxide Titanium Dioxide (Rutile) ' Lacquer Diluent Toluene Xylene Ethanol Isopropanol Butanol . Ethyl Acetate Butyl Acetate Butyl Cellosoli-e Methyl Ethyl Ketone Methyl lsobutyl Ketone lOO'.f 80f-t __ mm 9f 9 29 .-- 10.9 55 25 10 __ 15 ^ 20 MM 5 d) Rust-inhibiting primer b) Tint base that can-be pigmented to prepare a glossy finish c) Clear, exterior metal lacquer . d) 75-pcr cent nonvolatile in ethanol e) 25-per cent solution in solvent consisting of: Parts by Weight MM 100<* 56s 45 ' -- , 11 --. ' . ----- -- 1 M_ MM 55 85 195 '' -- 65 -- 55 ___ no M. 55 100 M- 75 -- 24 ' MM -- -- -- .----... MM MMM MM MM 160 11 MM 15 MM 95 60 -- Solvents . Per Cent Toluene 50 : Ethanol i Butanol 10 5 Ethyl Acetate 20 Butyl Acetate 15 /) Add indicated ingredients (60% of the non-drying alkyd) after other materials have been ground in a ball mill. . g) 65-per cent nonvolatile in xylene. \ $' 3 DSW 321969 STLCOPCB4073619 Clarity and adhesion are especially important whenever clear or pigmented coatings arc applied to metal surfaces. Shown below are example formulations for several metal lacquers: Ingredients R.S. Nitrocellulose (Wsec.)* R.S. Nitrocellulose (Vi-sec.)* R.S. Nitrocellulose (20-sec.)* Non-Drying Alkyd (609c NV) Santoute MHP -* ,, Shellac Solution (37% in methanol) Damar Solution (50% in xylene) Santiciser 160 or Dibutyl Phthalate Tricresyl Phosphate Toluene Xylene Butanol Ethyl Acetate Butyl Acetate Butyl Lactate ' * $5 9* - Peris by Weigh! 80 20 50 25 . __ 11 175 56 55 __ 115 -- .- 100 __ __ 7.7 ' 12 __ MO 40 __ 45 45 100 125 12 -- -- 45 __ 345 -- 25 85 200 -- ' 10** 100 __ -- -- 42 -- 32 150 -- 60 95 65 .-- a) General-purpose, clear, metal lacquer b) Lacquer with exceptional flexibility and adhesion for collapsible tubes, such as toothpaste tubes e) Clear, silver lacquer a) Clear, brass lacquer e) 75-per cent nonvolatile in ethanol Various other metal and specialty lacquers are illustrated below: Ingredients R.S. Nitrocellulose (t/i-sec.)* R.S. Nitrocellulose (Vi-sec.)* Coconut Oil Alkyd (Non Drying) Dibutyl Phthalate Diisodecyl Phthalate Sa.vtolite MHP Aluminum Powder ' Carbon Black Titanium Dioxide (Rutile) Dispersing/Grinding Agent Processed Clay Toluene Xylene ' Ethanol Butanol Ethyl Acetate Butyl Acetate Butyl Cellosoli'e Methyl Isobutyl Ketone Dichlorodifluoromethane ' ' fl) Hot-spray, exterior, metal lacquer b) Aluminum lacquer for a chrome finish c) Clear aerosol lacquer d) White aerosol lacquer e) 75-per cent nonvolatile in ethanol /) 60-per cent nonvolatile in xylene II* 22 __ 100 75 __ __ II 3 -- 170 16 45 ___ 105 65 * --,, -- 12k 13* Parts by Weight 50 50 125f __ 22 __ 30 __ __ 335 __ 55 40 115 155 100 __ 60 24 16 __ . -- __ . __ -- 20 __ 52 428 209 14* 100 __ 55 16 __ 12 __ 65 4 2 * r- -- __ ' A_ ___ 35 300 ` 590 4 OSVi 19l ) y) STLCOPCB4073620 Paper has become an important area for coatings and lacquers. Most protective-coatcd papers are used for cartons and labels. Lacquer films have also made washable wallpaper possible. Shown below are four example formulations of common paper lacquers. Nitrocellulose is the base for fingernail lacquers, of which formulation 19 is typical. - ' Ingredients R.S. Nitrocellulose (V^-sec.) S.S. Nitrocellulose ('/j-sec.) "* filacer* H-4055 Diethylene glycol ester ol terpene dibasic acid Sakticizer 160 or Dibutyl Phthalate Dicyclohexyl Phthalate Damar Resin (Dewaxed) Paraffin Wax . Santolite MHP Toluene ' Ethanol Butanol Ethyl Acetate Butyl Acetate 16* 100 72 28 '__ .-- __ __ 200 40 40 . 40 80 17k IB* Parts by Weight __ ' 100 __ 21 6 17 52 16 - --' 5 85 85 85 170 . . 100 __ -- 30 28 16 6 20 300 60 60 60 120 I9C 100 -- 50 -- -- -- 100 350 50 __ 200 150 a) Heat-sealing coating for paper. Dioctyl, dibutyl, and dicyclohcxyl phthalatcs, as well as tricresyl phosphate, can be interchanged as the platiciier with little effect in performance. The S. S. nitrocellulose would give a slightly better heat-seal test on glassine. b) Moisture-proof, heat-scaling paper lacquer c) Fingernail lacquer # Trademark of Cary ChemicaU. Inc. for vinyl chloridcvinyl acetate copolymers .' ' . . Nitrocelluloso-based heat-seal coatings arc widely used in the packaging of baked goods and other food prpducts. DSW321971 STLCOPCB4073621 One of the expanding applications for nitrocellulose lacquers is as coatings for plastics mater ials. Shown below are example formulations of various lacquers for plastics: Inqrsditnh R.S. Nitrocellulose (Vi-sec.) \ R.S. Nitrocellulose (5-6-sec.) Super Bcc\acilt* #1001 Oil-reactive phenolic resin Non-oxiduing Alkyd Resin Dioctyl Phthalate ` " SANTlci:tR 160 or Dibutyl Phthalate Dihydroabictyl phthalate . Partially Esterfied Pentaerithritol-Maleic Rosin Partially hydrogenated methyl ester of wood rosin Low-color blown castor oil Titanium Dioxide (Rutile) VM V P Naphtha Toluene Xylene Ethanol Ethyl Acetate Butyl Acetate Amyl Acetate Butyl Cellosolve Methyl Ethyl Ketone Methyl Isobutyl Ketone 20* 21* . 22` Parts by Weight 100 100 100 ... 100 __ ' * 25 100 30 -- _ - 25 62.5 ... 525 .... __ . .__ 90 155 __ - __ 370 ... _ _ 370 - __ ___ 1080 ---- ... .. '-- 30 100 too ... 420 -- 55 .. __ 770 23< .__ . 100 -- -- 25 -- 125 -- ' .. -- -- 290 -- 90 175 __ 30 -- Typical pigments and dyes can be incorporated by normal techniques. ) Lacquer with good adhesion to molded phenolic plastics b) Lacquer for acrylic plastics (automobile ornaments) c) Coating for ethyl cellulose plastics including the "soft" types d) Lacquer for Mylar-** and saran-coatcd cellophane, has excellent toughness, adhesion, and flexi bility. Dries in one minute at 100* C. s Trademark of Rekfcfcotd Chemical Industrie! * Trademark of E. 2. du Pone de Nemour* V Co. 6 DSW 321972 STLCOPCB4073622 ETHYL CELLULOSE Five basic properties make ethyl cellulose useful in many types of finishes and coalings: Color retention and stability Low-temperature flexibility . Selective solubility ' Alkali resistance As a result of these properties ethyl cellulose is used in a wide variety of coatings, including the following: . Cable lacquers Aluminum-foil coatings Paper lacquers . Gel lacquers Plastics lacquers Furniture finishes Sanding scalers Metallic finishes Decalcomania lacquers Floor-covering lacquers Bronzing lacquers Stop-off lacquers A wide variety of plasticizers is used with ethyl cellulose to develop its best properties to most satisfactorily meet the requirements of each particular application. Table II presents evaluations of various Monsanto plasticizers in ethyl cellulose with an ethoxy content of from 48 to 49.5 per cent: TABLE II--PERFORMANCE OF MONSANTO PLASTICIZERS IN ETHYL CELLULOSE (48- TO 4?.5-% ETHOXY) FILM Plasticiier (IS PHR) Yield Point IP*') Control (none) Dibutyl Phthalate Diphenyl Phthalate Tricrcsyl Phosphate Santicizer HO Triphcnyl Phosphate Santicizer E-15 Santicizer B-16 Santicizer M-17 Santicizer l'H Santicizer 8 Santicizer 9 Aroclor* 1242 Aroclor 1248 Aroclor 1254 Aroclor 1262 Aroclor 4465 6755 3625 5405 4550 5405 4550 4265 3485 4125 5475 4620 4620 4905 5475 6185 7110 8535 a) E = excellent G = good P = poor ' Tensile Strength (P`!) 8960 5120 7680 7465 8535 6685 7785 4905 7965 7750 6900 7325 7395 7540 7825 8035 9030 Elongation m 30 38 38 48 38 30 40 36 38 32 34 40 36 . 30 28 22 22 Hardness (releiive) 100 35 80 70 80 70 65 50 60 80 70 70 75 80 90 105 125 Aioclck: Moiuinto Chcnini Com piny Tridceml. Kcgiitcfcd in U.S. Pitent Office. Volatility E* G E E E E G G G E G G P P G E G Flexibility on Light Exposure E E G E E E E E E E E E G G G G P / STLCOPCB4073623 Ethyl cellulose-based lacquers improve the gloss and protect the appearance of high-quality wallpapers. Shown below are several suggested starting formulations for ethyl cellulose-based lacquers: Ingredionls Ethyl Cellulose ` Aroclor 1254 Aroclor 5460 Diphenyl Phthalate Tricresyl Phosphate . Dioctyl Phthalate ' Liquid poly (methylstyrene) ' Partially esterified pemaerythritol-malcic rosin Octylphenol Pentaphen* 65 (p-fert-amylphenol) Santocel* *FRC silica gel ' Antioxidant Titanium Dioxide (Rutile) Epoxy stabilizer Toluene -' Xylene Ethanol Butanol ' Butyl Acetate Cellosolve Butyl Cellosolve 24* 100f 64 504 -- -- -- -- -- -- '-- __ 0.4 200 4 __ 1120 --280 25*- 26* Parts by Weight 100s __. 100 __ 50 _ '. 1008 -- __ 72 ^_ 27* 100* ___ _. __ 54 27 2.5 -- -- -- 466 146 117 59 __ . 7.2 ,--- . -- -- _ 544 107 85 29 U. '-- 1.8 16 -- -- . * 428 ... 107 __ ` ... 28* 100* .... 22 ___ 100 .-- __ -- -- -- _ 178 _ 555 256 154 108 145 ) Alkali-resistant white lacquer f) 47.5-49.0-94 ethoxy, 10 cp b) Hard lacquer for rigid surfaces g) -n-5 49.0-94 ethoxy, 14 cp r) Tough lacquer for many surfaces h) 47.5-49.0-94 ethoxy, 22 cp d) Wallpaper lacquer i) 45.5-46.8-94 ethoxy, 200 cp c) Polystyrene lacquer (to minimise polystyrene crating, polystyrene solvents are kept at a minimum) * Tndcnirl of Pcnnaalt Chcmicala. Inc. Samtocu: Uxuintd Chemical Campanr TndcBirl. Rtgiautei in U.S. Patent Office. 8 0S**1S?4 0 / STLCOPCB4073624 Ethyl cellulose is widely used as a resin in protective-metal finishes, such as the following suggested starting formulations: Ingrediants Ethyl cellulose (45.5-56.8-% ethoxy) Super Bec\aciie # 1001 Glycerine ester of hydrogenated wood rosin Resimine* 881 melamine-formaldehyde resin Aroclor 1254 _ Aroclor 5460 " Tricrcsyl phosphate Triphcnyl phosphate Santicizer B-16 SANTONOX* antioxidant Ultraviolet-light Screener Epoxy Stabiliser - Xylene Isopropanol Butyl Acetate a) Chromium lacquer b) Aluminum-foil lacquer 29* 10CK -- 50 41 -- 1 1 1 1072 200 68 so*- 3|b farts by Weight too* -- - 33.3 33.3 ,_ e . -- 100<* 46.7 ,__ 10 10 267 66.7 -- __ 267 66.7 0 14 cp <0 10 cp 32*> I0CK 80 20 520 80 Solid plasticizers such as dicyclohexyl phthalate, triphenyl phosphate, and Aroclor 5460 are used in flow-back lacquers to give the desired flow-back characteristics. The flow-back is us ually achieved by brief heating to about 350F. Formulations 33 and 34 illustrate the use of solid plasticizers in typical flow-back lacquers based upon ethyl cellulose: Ingredients Ethyl cellulose (47.5-49.0-9i' ethoxy, 10 cp) Parlially-csterificd pcntaerythrirol-malcic rosin Aroclor 5460 or liquid poly(methylstyrene) Triphenyl Phosphate Dicyclohexyl Phthalate Carnauba Wax ` Toluene Ethanol 32 100 ___ 3016.7 3.3 240 60 Parts by Waight 34 100 16.7 31.7 __ 16.7 1.7 310 78 Kcsimekc and Saktosox: Monsanto Chemical Company Trademark*.. Registered in U.S. Patent Office. \ 32^ 5 OS'N 9 STLCOPCB4073625 The following suggested starting formulations illustrate the use of ethyl cellulose in two strippable coatings (Formulations 35 and 36) and in a hot-melt coating (37): \ Ingrtdi.nls 35* 36* 37* Paris by Weight Ethyl cellulose (47.5-49.0-% ethoxy.^50 cp) Paraplex* RG-2 polyester resin Super Bec^acite #2000 Non-oil-reactive phenolic resin Hydrogenated wood rosin Raw Castor Oil Hydrogenated Castor Oil Paraffin Wax (m.p., I35F) Dioctyl phthalate Aroclor 1254 Soy-bean lecithin Octylphenol Stearic Acid Pentaphen Non-leafing aluminum Heptane Toluene Ethanol Isopropanol 100 13 .' ... 61 __ __ __ 22 8.7 _ 2.2 114 326 196 65 65 100 ---- ** . ---- __ ' ' __ 100 2 2 __ __ 306 184 61 61 100 -- 100 133 __ 133 167 33 .... __ -- .__ __ _ -- a) Aluminum colored b) Solvent based . c) Low moisture permeability, good heat-sealing characteristics, and excellent low-temperature flexi bility _ The use of ethyl cellulose in size emulsions is shown in the following formulation, which is made by dissolving the resins and plasticizer in the solvents and the emulsifying agent in the water. The lacquer phase is added to the water phase with agitation. The resulting crude emulsion is homogenized by one pass through a Premier Eppenbach or Montar-Gaulin mill. The resultant finished emulsion is. filtered through a 30-mesh cloth. Ingredients Lacquer Phase Ethyl cellulose (47.5-59.0-% ethoxy, 100 cp) Durei** 550 Phenol-Formaldehyde Resin Triphenyl phosphate Xylene . Hi-flash Naphtha Butanol Water Phase Potassium Olcate Water 38 Paris by Waight 100 20 70 270 160 50 .. 5 325 "Tiufenait of Rohm & tUu Co. of Hooter Chemical Corp. \ 10 DSW 321976 j' ft STLCOPCB4073626 0 CELLULOSE ACETATE-BUTYRATE . Cellulose acetate-butyrate resins display excellent low-viscosity properties, making attainable high-nonvolatile-content lacquers for spray, roll-coat, or brush application. On evaporation of the solvent, these lacquers produce films with the following characteristics: . " . Adhesion Clarity Toughness Heat resistance Solvent resistance . .. Cellulose acetate-butyrate can be utilized in a broad range of air-curing coatings, including the following: Clear and pigmented metal lacquers. Paper and textile coatings and impregnants Plastics lacquers Hot-melt coatings Wood lacquers Protective pcclable coatings Glass and rubber coalings . Cellulose acetate-butyrate resins are available in 17-, 27-, 38-, and 50-weight-per cent butyral content. Since the application of these surface coatings cover such a .wide spectrum, the selec tion of the best combination of cellulose acetate-butyrate resin and plasticizers for a specific use poses complex problems. The performance of various Monsanto plasticizers in the four com mon cellulose acetate-butyrate resins is shown in Table III. II DSW 321977 STLCOPCB4073627 o> Ok <s 0 oM* *% M rf-4 Mw rt f| Ci3O2 oooooooooo no^orvokooOoo'OoNoyoNovj u. * S 2 %n oOkO'TOO^'OOO^OOOOcO'O ca g N-< ft rt Cr*ft N *x oT r- Ui oO< UtnI CO 72S e ^o*> oooooo o oo ooooooo o(^ocooOokOoeOofo^^oOoeOocoOto^^oo^oOo^ oco 3? p ui O z ionf Ui N O Hl/> 5 o z <lzo/l 2 LL O ui Oz < 2 fi 2 oUJf a. tn5 1 cr*t rt oro erot iI o^or kHONYNrNOrOtfcHO'OtrHtrHt \ 1 ^O^f 1 SI sMi n x a J*52 r* *ci *3*. .6c rQ= ft ft ft -Ca O-a* *M. .oc 73 & ft JO p* ft H 2 if<i P, .^NH\ <5 A- (/] *> (4% f1t1i g cpz</} OSi H D Pz to< O^^ h ex *cc_w I- a- KN JE3 o, 'C H <o C/> J ! I ) o DSW 321978 STLCOPCB4073628 Shown ueiow arc several example formulations for important cellulose acetate-butyrate lacquers: ' Ingredients 39* 40* 41* 42* PrH by Weight Cellulose Acetate-Butyrate (*/;-sec.) Ambeiol* 820 hard rosin-modified maleic resin Acrylic Ester Resin FDC SSSB** (50% n.v.) -- Aroclor 1260 Aroclor 1262 Aroclor 5460 Tricrcsyl Phosphate SaNTICIZER 409 Santolite MHP . Solvesso*** 100 ' Toluene Ethanol Butanol Isobutyl Acetate _ Acetone Methyl Ethyl Ketone Methyl Isobutyl Ketone Dow Corning 200 Silicone Fluid (1000 cs) 100 75 .__ -- 240 60 25 -- ' 100 79 100 __ ' ... __ 51.6 __ - __ 415 105 264 __ -- _ `_ _ -- .... 50 __ 200 50 __ 50 50 __ -- a) Low-cost, flame-resistant lacquer for paper coating and impregnation 100 -M 42 '-- - 25 - ` 25 -- --' __ 250 560 417 __ 167 85.5 -- b) Paper lacquer with exceptional adhesion to inked surfaces c) High-gloss paper lacquer . i) Lacquer for cellophane, cellulose acetate-butyrate, and cellulose acetate e) General-purpose metal and metal-foil lacquer (gold, silver, aluminum, and chromium) 43` lO'O __ _ 22 __ __ 22 -- 13 ___ 51 286 14 57 -- __ , __ 106 0.07 Hot-melt coatings constitute an important area of application for J^-sec. cellulose acetate- butyrate lacquers. The use of dioctyl phthalate as the standard plasticizers for hot-melt coat ings is shown in the following formulas: ' Ingredients 44* 45> 46' Peris by Weight Cellulose Acetate-Butyrate (Vi-sec.) Aroclor 1260 Dioctyl Phthalate Titanium Dioxide (non-chalking rutile) Calcium Carbonate (precipitated) SantowhiteI Powder Refined Antioxidant Odor-masking Agent 100 ___ 67 33 133 0.3 0.03 1_0_0_ 66.5 __ 0.17 -- 100 80 20 .... 0. . a) Pigmented fiberboard knife-coating for exterior exposure b) Clear melt coating for heavy, one-coat film: economical (no solvent loss) and low application hazard c) Clear, low-cost, flame-retardant melt coating . . 9 Tndcnitt of Rohm & Haas Co. 99 Trademark of France. Campbell Darling, Inc. Trademark of Eeso Standard Oil Co. ^ fSaxtovhiir ; Monsanto Chemical Company Trademark. Registered in U.S. Patent Office. 13 DSW 321979 STLCOPCB4073629 Strippable spray coatings are increasingly useful in various industries. Cellulose acetate-butyrate provides an excellent base for coatings of this type. The following are two typical applications: Ingredients \ 47* 46b Parts by Weigh! Cellulose Acetate-Butyrate (Vi'see.) Aroclor 1260 Aroclor 5460 .^ Tricresyl Phosphate Santicizer 409 Dioctyl Sodium Sulfosuccinate Sodium Dichromate Toluene Ethanol Isopropanol Butyl Acetate Acetone Methyl Ethyl Ketone . 100 60 -_ SO -- 1.6 132 6._3.5 26.5 47.5 47.5 100 __ 27.8 -- , 45 9 0.7 3_12 102 -- __ 97 a) Flame-resistant, brushablc coating b) Temporary, easily strippable coating for shipping tools and machine parts containing corrosion inhibitors The following fcumulation illustrates the use of cellulose acetate-butyrate base as a wood filler and prefinish: Ingredients Cellulose Acetate-Butyrate Aroclor 5460 Magnesium Silicate Toluene . Butanol ' Butyl Acetate (V^-sec.) ` 49 Parts by Weight 100 214 -642 85.7 71.5 314 To provide protective and decorative coatings for materials such as glass, rubber, and leather, various specialty coatings have been developed. The following formulations are characteristic cellulose acetate-butyrate lacquers: Ingredients ** Cellulose Acetate-Butyrate (Vi-sec.) FCD JJ5B (50% n.v.) Plas\on* 3115 (60% n.v.) Urea-formaldehyde Resin Santicizer 409 Dow Corning 200 Silicone Fluid (1000 cs) Santowhite Powder Refined Antioxidant Toluene Xylene Ethanol ` Butanol Butyl Acetate BO> i100 _, 74.5 74.5 __ l.i 417 178 178 89 Parts by Weight ' 5*1 b 100 ' 21.8 -- 20.3 0.07 MM 216 144 57 57 117 ` a) High-luster lacquer with excellent adhesion to GRS rubber ' b) Clear glass lacquer with exceptional adhesion to all types of glass even after water immersion Tniknul of Allied Chemical Corp. ' 14 DSW 321980 STLCOPCB4073630 CELLULOSE ACETATE ' The following properties of cellulose acetate make it adaptable for many specialized lacquers: Toughness - Clarity . Durability Stability to heat, light, weak acids, and oils . Good dielectric properties . ' : These properties make it useful for metal, wood, paper, textile, leather, and plastics coatings. Plasticizers improve the flexibility, suppleness, and other physical properties of cellulose acetate films. . In Table IV are presented performance data for several Monsanto plasticizers in cellulose acetate molding compositions. . TABLE IV--PERFORMANCE OF MONSANTO PLASTICIZERS IN CELLULOSE ACETATE COMPOSITIONS PV lUuatliSiwciiaiAuri (51.5 PHR unless otherwise specified) Solution Temp. (*C) Dimethyl phthalate 120 Diethyl phthalate 140 Santicizer M-17 148 Santicizer E-15 148 Santicizer 8 133 Santicizer 9 153 Triphenyl phosphate (42.5 PHR) 180 Herdnoss *t TO'C Rockwell M ScaU .32 ' 15 65 50 75 90 81 Flexural Strength , (Ib./sq. in.) 5840 5680 7110 6930 6860 9160 9020 Water Absorbed in 48 hr. m 1.14 1.20 0.77 0.97 0.94 0.85 1.17 Shown below are two example formulations of cellulose acetate lacquers: Ingredients 52* Cellulose Acetatec Alkyd Resin Santicizer M-17 Zinc Oxide Phosphoric Acid (aids adhesion to metal) Toluene Ethanol Butanol Methyl Acetate Nitromethane I-Nitropropane 100 40 50.7 80 0.05 312 176 38.7 __ 244 176 <t) White metal lacquer for interior use b) General-purpose spray lacquer c) 52.5-53.5 % combined acetic add, low viscosity Parts by Weight 53h 100 30 37 0.05 372 206 54.4 137.5 287 206 15 DSW 321981 STLCOPCB4073631 Paper and cloth coatings are important areas of application for cellulose acetate. Shown below are three suggested starting formulations: . Ingrsdiants Cellulose Acetate Triphenyl Phosphate Santicizer M-17 Santicizer E-15 Santicizer 1-H Water Ethanol . Butanol Methyl Acetate Ethyl Acetate Acetone " \\ # 54- 100* 18.5 *16 __ ' ' -- __ - 108 ---- . __ 660 5S*> Parts by Weight 100i --' --- 67 --- 67 100 - -- 550 -- .. ' 56* too* 60 -- -- - 50 '-- too 40 650 -- :-- a) Heat-resistant paper lacquer b) Greaseproof food-packaging lacquer c) Flame-retardant, stain-resistant doth coating d) 55-56-% combined acetic acid, low viscosity e) 54-55-% combined acetic acid, high viscosity Cellulose acetate lacquers impart the best adhesion, gloss, and durability on cellulose acetate plastics. The use of these lacquers minimizes plasticizer migration. Shown below arc some char acteristic formulations: . ' Ingredients 57* Cellulose Acetate Dutcz 500 Santicizer E-15 Santicizer M-17 Santolite MHP Water Toluene/ Ethanol Ethyl Acetate Methyl Cellosoh-e Methyl Ccllotolve Acetate Acetone 1-Nitropropane 100<* __ 100 260 156 __, 740 -- ' _- <r) Plasticizer-migration-resistant lacquer b) Cellulose acetate plastics lacquer c) Gel dipping lacquer d) 55-56-% combined acetic acid, low viscosity e) 52.5-55.5-% combined acetic acid, low viscosity {) Add toluene slowly 58>> 59b Parts by Weight 1004 a. 20.5 __ ___ . 156 41 . ... __ 116 275 116 1004 . 60 ` __ 40 __ __ 226 68 __ __ 195 455 195 60c 100e __ __ 82 151 __ 415 149 102 a___ -- 16 DSW 321982 STLCOPCB4073632 MONSANTO PLASTICIZERS IN VINYL COATINGS I POLY{VINYL ACETATE) Surface coatings based on poly (vinyl acetate) fulfill a variety of requirements and are char acterized by: Ease of application . Fast drying Good adherance High gloss . Transparency Resistance to water, fats, and oils . Poly (vinyl acetate)-based formulations are used extensively in the following applications: Cloth coating Paper coating and impregnation . Paint primers and sealers Interior and exterior paints Greaseproof, oil-resistant coatings Wall-patching compounds A wide selection of plasticizers for poly (vinyl acetate) and its co-polymers is available. Gen erally these plasticizers increase flexibility and lack, increase water and grease resistance, and lower heat-sealing temperature. Performance evaluations of several Monsanto plasticizers in poly(vinyl acetate)-emu!sion adhesives are listed in Table V. , 17 DSW 321983 STLCOPCB4073633 I 0 18 DSW 321984 STLCOPCB4073634 The following suggested starling formulations illustrate the toughness, durability, and grease resistance imparted to paper and cloth coatings by poly (vinyl acetate): Ingredient* *1* Poly (vinyl acetate) emulsion Elvanol* 7130 Poly (vinyl alcohol) (I0Cr Aq. Sol'n.) Methyl Ester of partially hydrogenated wood rosin Santicizer 160 or Dibutyl Phthalate Santicizer 141 _ Calcium carbonate (fine ground) Titanium f>ioxide (Rutile) - Tamol** 731 Dispersing Agent (25l7c Aq. Sol'n.) Water Polypropylene Glycol (1200 molecular weight) 100-* -- 8 17 *.e> __ 9.4 -- ' Ml Parti by Weight 100* . JO ' __ __ 8.25 119.25 1J.25 2.10 J4 1 Properties . Total Solids, per cent Viscosity (26'C), cp Pigment : Binder Ratio PVAc Resin : PVA Resin Ratio PVAc Resin : Plasticizer Ratio . a) Artificial-leather coating for knife-coating of cloth or paper b) Pigmented greaseproof coating for flat board c) Greaseproof coating for flexible board .. d) Polyco*** 117H e) Cclva S-55 or Elvacet* 81-900 65 1600 2:1 18 : 1 6.6 : 1 63* 100* JO .... __ 13.75 96.75 10.75 1.80 J4 1 65 2700 1.5 : 18 : 1 4:1 Preparation of 61 . ' -' Blend plasticizer and wood-rosin methyl ester. Then add poly(vinyl acetate) emulsion. Preparation of 62 and 63 . 1. Frepare a stock solution of poly (vinyl alcohol) by slurrying in water at room tem perature with good agitation. Heat for 30 to 40 minutes at 185 to 190F. Add water for solids control as required. 2. Continue stirring, add the plasticizer, polyethylene glycol defoamer, and Tamol 731 pigment disperser. 3. Add the pigments, stirring until dispersion is complete. 4. Add the poly (vinyl acetate) emulsion and stir until a homogeneous mixture is obtained. * Trademrk of E. I. do Pont dc Kemourt ** Trademark of Rohm V Hail Co. *'* Trademark of Tbe Borden Co. Co. \ 19 DSW 321985 STLCOPCB4073635 - A paint thinner and a quick-drying primer sealer for masonry and wallboard coatings are exemplified by the following suggested formulations: Part I Gelva poly (vinyl acetate) Emulsion TS 22 Santicizer 160 or dibutyl phtbalate -- M4 65*> Pri by Weight 100 100 8 8.8 Part II Water ' Carboxymethyl Cellulose (High-Viscosity Type 70) Burtonite* X 90 guar-seed gum 58 1.25 0.75 40 0.6 __ Part III Water Tamol N dispersing agent Tetrasodium pyrophosphate Titanium Dioxide (Rutile) Mica Talc 260 80 ,, 0.3 __ 0.3 15 __ 30 _ 30 a) Paint thinner b) Pigmented primer-scaler: quick drying, non-penetrating, and insoluble in mineral spirits Preparation 1. Prepare Part I by adding the plasticizer at a moderate rate to the emulsion with stirring. Continue agitation for 20 to 30 minutes or until a smooth, uniform mixture is obtained. 2. To prepare Part II, stir the carboxymethyl cellulose into the water, continuing agitation until complete solution occurs. For the thinner, add the guar-seed gum and stir until a completely homogeneous mixture is obtained (about 10 minutes). Use of water at 70 C (160F) accelerates solution of the thickeners. Stir the plasticized emulsion (Part I) into the thickener (Part II). 3. a) Add the remaining water to the thinner (formulation 64). ^. b) For the sealer (formulation 65), dissolve the dispersing and dcflocculating agents into the water. Stir in the pigments, and mix or grind the slurry. Add the sealer base (the mixture of Parts I and II) and thoroughly mix with the pigment slurry. Tndcmirt of Tbc Burwcuie Coopiny 20 DSW 321986 - STLCOPCB4073636 Poly (vinyl acetatc)-emulsion paints for interior and exterior surfaces are suggested in the following formulations: Ingredients - . Pert I Water Burtonite X-90 guar-seed gtim Pen II Cclva Poly.(vinyl acetate) emulsion TS 22 Santicizek 160 or Dibutyl Phthalatc . Part III Water Tamol 731 (1% soln.) Dispersing Agent Carboxymethyl Cellulose (Low-Viscosity Type 70) Chromium Oxide, opaque Titanium Dioxide (rutile, 30%: calcium sulfate, 70%) Titanium Dioxide (rutile) Mica e) Light-green, interior, emulsion paint b) White, exterior, emulsion paint 66* 67t> Farts by Weight 41.0 0.8 19.8 0.68 100 12.2 100 8.2 110 6.5 1.2 6.5 66 33 . 14.6 67 1.2 0.9 JJ.4 29.6 Preparation ' Parti Add the guar-seed gum to the water with high-shear mixing until a homogeneous solution is obtained (about 10 minutes). . Part 11 While stirring the poly (vinyl acetate) emulsion with a high-shear mixer, slowly add the plas ticizer. Stir for 20 to 30 minutes after the plasticizer is added or until the mixture becomes uniform. Add the plasticized poly(vinyl acetate) emulsion (part II) to the guar-seed-gum solu tion (part I), and stir for 10 minutes or until homogeneous. Part 111 . With the colloid mill operating, sift the carboxymethyl cellulose into the water and dispersingagent solution in an aluminum or stainless-steel vessel. Mix until dissolved. Slowly sift in pig ments in the order listed. Grind to desired fineness. Add paint base and stir for 10 minutes. Filter through an SO-mesh screen. 0 '. ' 21 DSW 321987 STLCOPCB4073637 The following suggested formulation is for a polyfvinyl acetate)-based latex wall-patching compound: - Ingredients ' 63 . Parts by Weight Poly (vinyl acetate) emulsion Hydroxyethyl Cellulose (75% n.v.) Tricresyl Phosphate #6MetTO'i^ite " Water Ethylene Glycol L too 50 5 772 3 35 Preparation - Mix the poly(vinyl acetate) emulsion and the hydroxyethyl cellulose solution in a pony mixer until completely dispersed. Stir in the water and ethylene glycol. Mix for 5 minutes, and add the Mctro-Nite in 5 equal portions, allowing each portion to wet down thoroughly before adding the next portion. Add the tricresyl phosphate and continue to mix for 30 minutes. Properties Consistency Nonvolatiles, per cent . Pigment : Binder Ratio, weight Density, lb./gal. Pasty - spreadable and workable 81 . 12.2 : 1 16.6 Vinyl acetate is often copolymerized, as for example, with vinyl pyrrolidone. The following common Monsanto plasticizers are compatible with vinyl acetate-vinyl pyrrolidone (70/30 to 30/70) copolymers: . ' . Dimethyl Phthalate. Dibutyl Phthalate Santicizer B-16 Santicizer E-1S Santicizer 141 Santicizer 213 Santolite MHP . ( Dimethyl Phthalate and Santicizer E-1S are particularly effective in imparting flexibility to this copolymer. The following starting formulation gives an anti-tarnish coating that dries to a clear, smooth film without "orange peel" and that can be simply washed off with a synthetic- detergent solution: Ingredients Vinyl Acetate/Vinyl Pyrrolidone Copolymer (70/30) Santicizer B-16 Isopropanol Propellant 11* Propellant 12* * For non-aerosol applications substitute methanol for propellant. " W Parts by Weight too 5 . 145 375 375 22 DSW 321988 j STLCOPCB4073638 POLYVINYLCHLORIDE) ' Poly (vinyl chloride) and its copolymers are widely used in protective coatings. In general, coatings based on poly(vinyl chloride) display the following characteristics: ' . .. . . . ' Hardness Flexibility Abrasion resistance ..Chemical and water resistance Greaseproofness . Electrical resistance Nontoxicity Odorlessness Taslelessness Flame retardance . Poly(vinyl chloride) coatings may be applied in any of the following forms: Solution. Solvent must be volatilized to develop strength. Latex (emulsion). Water must be volatilized. Short bake helps develop optimum properties. Plastisol. No volatile solvent. Curing temperature: 300-350F. Organosol. Some volatile solvent to control sprayability or coatability. Curing tempera ture: 300-350F. ` . Powder (fluidized bed). Product to be coated is heated to high temperature and suspended in fludized poly (vinyl chloride) powder. Since the applications for poly (vinyl chloride) are so broad, only solution and latex coatings are described in this bulletin. Other Monsanto literature discusses plastisols and organosols in detail. Monanto offers more than 70 plasticizers to enable the poly(vinyl chloride) formulator to develop the balance of characteristics required to meet his requirements successfully. The per formance of some of the plasticizers in poly (vinyl chloride) is indicated in Table VI. \ 23 SW 321989 STLCOPCB4073639 1CO r* -- a" ,?-S Q " _ mCK m m y) N N fi N OHf-Or;t *N Q 0^0 c VH o o> o ^ * q r- o H H * . N. 6- ^H *> v% t f _. OTk h fj d q o k d v <r <| o oo Tk O . H ri d ** t2> _S s<. m ut~ X CO r* <o O o H r r** A t- rt r rt-- r*-e* t- >o CoO HOk u> o' Hi N o rO~ rvot t~ o r~ r~ o --1 t- A AA OIz-- 9~ui <sZp ooJ _j OI 2O oUL > Z LU o >, Z <o 2 Cl. cm 2s > UI co < J> <0 o < S H. >3 H o v> o H rt oo o CO 00 H H d -J o o orO VV53 OCO O oo > -I o d o o o d o o. v o Ok oooo ood o 2 *-* t o a >* --- Eo (i fi ^ ri ri n r i*i ^ n IIIIIIIIIIIII q v* eo oo ve - o co CO H 00 q co e* - X o 04 41 *2 a 2 3 _Ce* 3 * fr s s SO.. ^ O. ,, >KN Uo o w>u 8 f QQQ >H p *3 0( H y P < co -4 N c H 0 pz < co N tC H D P Z < CO H oo H D Pz < CO eft O O cn V5 `SO < CO *4 V3 h ?^. co *= 3 k< .uy H 4 N G Pz < to " H G p z K jC P S* 5 o * -- PP * M 14 G P z CO 24 dS\N 32199 & STLCOPCB4073640 Solution Coatings Because of their excellent permanence and performance characteristics, poly (vinyl chloride) resins are ideally suited for metal coatings. Like other coatings, however, they require a suit able primer for satisfactory adhesion. The following formulations exemplify the versatility of Monsanto plasticizers in the manufacture of poly (vinyl chloride) solution prime coatings: Ingredients 70* 71* 721- 73* Parti by Weight VinyJite* VMCHJ Vinylite VYHtt* Exon** AW* Esterified Copal Resin Tricresyl Phosphate Santicizer 409 Dioctyl Phthalate Red lead pigment Blue lead pigment Zinc Oxide (colloidal) Titanium Dioxide Propylene Oxide Toluene Xylene Methyl Isobutyl Ketone Ethyl Amyl Ketone Cyclohexanone _ " . - 2.5 37.5 ' 4. . '_ 18 __ 25 ' __ 216 216 ' ai -- 100 __ 16 *-- __ 25 ... -- *14 -- no no __ . a) Air-dry or low-bake primer (200* * 300*F for a short time) ---- ' -- -- 100 100 -- --- -- -4 -- 12 -- --- 140 -- -- ---- -- ' --. 4 188 162 -- 40 100 162 8 40 " b) General-purpose primer e) High-temperature-bake primer (350" - 375*F) d) Vinyl chloride copolymer (metal-adhesion type) Trademark of Union Carbide Corp. Trademark of Fireatone Plastica Co. / \ * Vinyl solution primers end finish coatings impart attractive, durable protection to numorous metal products. 25 DSW 321991 STLCOPCB4073641 A variety of solution formulations may be used in intermediate and final coats as illustrated below: .- . Ingredients Exon 450f Vinylite VAGHf Vinylite VYHHf Vinylite VMCHI Urea-Formaldehyde resin Rosin WW Liquid epoxy resin Tricresyl Phosphate Santicizek HI Dioctyl Phthalate Diisodecyl Phthalate Santicizer <09 Blown Castor Oil Titanium Dioxide Zinc Oxide Cuprous Oxide Aluminum pigment Antimony Oxide Propylene Oxide Stabilizer Toluene Xylene Methyl Isobutyl Ketone Cyclohexanone 74* v 75*> too mm -- . --. ---- . ^-- 'to ' ... ' - __ . ---- -- - . .... 45 204 __ 204 -- * 100 .... -- 19 9 __ 1.25 42 36 17.5 ... .... 160 40 160 40 a) Intermediate coating b) General-purpose industrial coating . c) Metal finish d) Corrosion-resistant coating e) Anti-fouling coating (MIL P-15931) /) Vinyl chloridc-vinyl acetate copolymer 74>> 77*> 78' Parts by Weight 79<> 100 * 50 _ 50 __ . -- IS 10 __ . 67.1 100 __ . - 18.7 -- 14.2 - -- ' -- - __ - 13.4 7.5 67 __ 193 48 193 48 .... . __ __ 45 .... __ 255 255 -- .... 57 .__ -- __ ... __ ---- 140 84 56 6.7 __ 100 __ _ __ __ __ 6.7 13 127 __ 435 -- SO' .... too __ __ 100 -- 3S __ -- .... 1000 __ .... 220 350 -- . . . When extreme corrosion resistance is required, the use of Aroclor plasticizers is suggested: for imparting resistivity to chemical attack, they are unsurpassed. Independent evaluations of the chemical resistance of vinyl chloride-vinyl acetate copolymer paint, modified by eight types of materials (alkyd resin, phenolic-chinawood oil varnish, ester gum-linseed oil. varnish, Aroclor 1254, dioctyl phthalate, tricresyl phosphate, polymeric plasticizer, and acrylic polymer), showed that Aroclor 1254 has the "best all-around chemical resistance, failing badly only in the gas oline test." Paints were sprayed onto solvent-cleaned, unprimed, cold-rolled-steel panels, which were then immersed in seven types of solutions until failure. The data in Table VII, excerpted from the November 1955 issue of OJJieial Digest of the Federation of Paint and Varnish Production Clubs, compare the chemical resistance imparted by Aroclor 1254 and by dioctyl phthalate. -1 ii ( 26 DSW 321992 STLCOPCB4073642 (gf ( ]> I - TABLE VII--COMPARATIVE CHEMICAL RESISTANCE OF PLASTICIZERS IN VINYL CHLORIDE-VINYL ACETATE COPOLYMER PAINT Plasticiser Dioclyl Phthalate (V.) AROCLOR 1254 m 10% Sodium Hydroxide (days) ioy. Hydrochloric Acid (hours) Tima to Failure in Corrosivei Media Gasoline (day.) 5% Sodium Hypoehlorila (days) ioy. Acetic Acid (hours) 10 ' -- 10 25 .25 40 __ 50 ) End of test 120* 120* - 60 120* 60 120* 92 . 168* 24 120 . 24 96 0.4 5 0.4 0.4 0.4 0.4 4 15 4 14.5 4' 11 84 168* 84 120 48 100 Linseed Oil Fatty Acids (days) 60 90* 27 90* 22 60 1*/. Tide at IWF (days) 21 22 25 22 25 22 In other corrosion-resistance tests of poly (vinyl chloride) plastisols, containing 70 parts plas ticizer per 100 parts resin, a formulation that contained 1 part Aroclor 1254 to 3 parts dioctyl phthalate was much more resistant to 15 per cent nitric acid at either 23 or 50C for six months than a compound plasticized with dioctyl phthalate alone. The plastisol modified with both Aroclor 1254 and dioctyl phthalate was also more resist ant to 25 per cent chromic oxide at 50C for four weeks and was equivalent at 23C for six . months in comparison with the dioctyl phthalate-modified vinyl plastisol. Coatings are frequently based on combinations of vinyl chloride-vinyl acetate copolymer and nitrocellulose resins, as exemplified by the following suggested starting formulations: Ingredients Blacar H-4055 R.S. Nitrocellulose (Vi sec.) Tricresyl Phosphate Dioctyl Phthalate Epoxy resin Titanium Dioxide (non-chalking rutile) Carbon black Toluene Xylene n-Butanol Ethyl acetate Butyl acetate Cellosolve Acetate Methyl Isobutyl Ketone Methyl Amyl Ketone 81* 50.2 49.8 59.2 '-- -- 58.8 5.5 557 52.4 25.9 58.5 142.5 --. .-- 52.4 82h Parts by Weight 83* 40 60 -- 22 5 -- __ 200 100 __ __ 124 __ 25 50 ' ' 50 50 -- 55 -- 50 __ 175 100 .__ __ 125 50 50 -- c) Gray automobile lacquer b) Clear indoor lacquer c) White indoor lacquer: apply over suitable primer and bake Vi boor at 150*F 27 DSW 321993 STLCOPCB4073643 The following formulation illustrates a nontoxic paperboard coating for food packaging: Ingradiants Vinylite VYHH Vinylite VMCH Vinylite VAGH Santicizer 141 Acetone Methyl Isobutyl Ketone \ 84 Paris by Weight 80 10 10 25 300 . 175 Strippable lacquers have become increasingly important as protective coatings for a variety of materials. Shown below are two formulations (85 and 86) that illustrate this type of coat ing and one (87) that exemplifies a sprayable coaling with good webbing characteristics: Ingredianft 85* Exon 468 vinyl chloride-vinyl acetate copolymer 27 Exon 470 vinyl chloride copolymer (metal-adhesion type) 3 Exon 48! vinyl chloride-vinyl acetate copoylmer 70 Vinylite VYHH vinyl chloride-vinyl acetate copolymer __ Santicizer 160 __ Santicizer 409 ' 31 Dioctyl Phthalatc 16 Dioctyl Adipate 14.7 Aroclor 1254 __ Prime pigments Titanium Dioxide . 27 __ Stabilizer 12 Propylene Oxide Socony White Oil #318 6 __ Toluene ' 70 Xylene __ Methyl Ethyl Ketone - 312 86* Paris by Weight __ 100 11 ' -- -- -- -- 5.5 __ _ 6.7 24* 254 a) Sprayable waterproof coating b) Lacquer with good spray qualities and quick-drying, hard, and opaque film c) Sprayable web coating - ' 87* _ ... _ 100 B0 -- T2 -- -- -- -- _ 118 --. 294 e 28 DSW 321994 STLCOPCB4073644 Latex (Emulsion) Coatings Whenever the characteristics of poly (vinyl chloride) and its copolymers are desired, but the hazard of flammable solvents cannot be tolerated, the use of a poly (vinyl chloride) latex (emulsion) is indicated. Shown below are three suggested starting formulas: \ l I t i tI Ingredients - Ceon* 251 Geoit 352 Geon 526 . * Dioclyl Phthalate (65% emulsion)* Dioctyl Adipate (65% emulsion)* Santicizer HI (65% emulsion)* Santicizer 409 (65% emulsion)* Aroclor 1254 (45% emulsion) Goodrite* K-710 thickener (5% solution) Mobilcer** R microcrystalline wax (45% emulsion) Keltex*** thickening agent (2% solution) Titanium Dioxide (50% dispersion) Calcium Carbonate (50% dispersion) Antimony Oxide (50% dispersion) Color Pigment (50% dispersion) Iron Oxide (50% dispersion) Dibasic Lead Phosphite (50% dispersion) 86* 8?h Parts by Weight 1004 20 , 15 _. 15 -- 1 -- -_ 30 15 ' -- " __ || ' . 1004 10 -- -- 5 I __ 20 go* 1004 . --_ 25 7 -- -- 250 45 15 -- 5 *>) Thin fabric coatings. Excellent for bridge coats on loosely woven fabrics before subsequent spread coating with an organosol or plastisol b) Jute-felt floor covering or automobile-trunk liner c) Flameproof coating: complete immersion then squeeze rolls (patented) d) . Solids e) Typical Plasticizer Emulsion: Ingredients Parts by Weight Plasticizer 65 Water . 33.4 Oleic Acid 1.25 Ammonium Hydroxide (28%) 0.35 i Trademark! of B. F. Goodrich Chemical Co. for ttolyfvinyl chloride) reiiru I Trademark of Socony Mobil Oil Co. i '* Trademark of Kclco Co. *i i \ 29 DSVV 321995 STLCOPCB4073645 The use of vinyl chloride-vinylidene chloride copolymer latexes in fire-retardant, intumescent coalings for wallboard and acoustic tile is shown below. The use of the solid plasticizer, diphenyl phthalate, improves the viscosity stability of formulation 91. Ingredients. \ Part I Monoammonium Phosphate - Dicyandiamide Pentaerythritol Titanium Dioxide (Rutile) Diphenyl Phthalate ' Anionic Wetting Agent. Acid Stable Water ,, 91 Parti by Weight 56 10 22 12 3 1.25 47-14 ' . 56 10 22 12 -- -- 46-61 . Part H ' Dow Latex 744-B (vinyl chloride-vinylidene chloride copolymer) 40 Santicizer 141 or Dioctyl Phthalate Suspension Agent, Acid Stable _- Anionic Emulsifier, Acid Stable -- 42.8 10 0.6 1.2 Preparation 1. Mix the intumescent agents, pigment (and plasticizer and wetting agent for formula tion 91), and water. Disperse with two passes through a high-speed stone mill. 2. Add the latex (plasticized for formulation 92) with medium stirring. The applications of vinyl latex coatings are increased by the addition of intumescent and fire-rotprdant agents. 30 DSW 321996 c STLCOPCB4073646 I . ! i }. J I i tt 1 f I t i j (.9 it . j j \ i | I 1 . | i ' . > MONSANTO PLASTICIZERS IN RUBBER COATINGS ' CHLORINATED RUBBER Chlorinated-rubber-based coatings are widely used because of their resistance to corrosive agents, moisture, fungus, mold, and other destructive agents. Consequently they are used in such applications as the following, which require extreme resistance to the above deteriorating agents: ' - Masonry Flame-retardant finishes Chemical plants Railroad equipment Marine equipment Swimming pools Food-processing buildings ' Highway paints . Monsanto manufactures many plasticizers that are useful with chlorinated rubber. Particularly beneficial are the Akoc-lor compounds, which enhance the chemical resistance of the chlor inated-rubber-based finishes. Table VIII indicates the utility of various Monsanto plasticizers in chlorinated rubber: ' TABLE VIII--EVALUATION OF MONSANTO PLASTICIZERS IN CHLORINATED RUBBER Good adhesion to ' Resistance to Plasticiser Alum- Sieel inum Cop per Tr#injHe Seeled Wood Cello phane 10% 5% Sodium Hydro- Sodium Chloride chloric Hydrox- Acid idc Water Sward CcldHerd- Chech nets Resitfa nco (cycles) Aroclor 1254 -- -- -- X -- X X X X X 35 3 Aroclor 1260 -- -- -- X -- X X X X X 40 4 Aroclor 5460 XX--X -- X X X X 22 2 Dibutyl Phthalatc X--X-- -- -- X -- X X 53 5 Sakticizer B-16 -- -- X -- X .-- X -- X X 45 7 Tricrcsyl Phosphate X -- X X X -- X -- X X 56 5 Triphenyl Phosphate -- -- X -- X -- X -- *-- -- 60 4 Santolite MHP 28 . 2 X--indicates good adhesion or resistance Although chlorinated rubber is unaffected by acids, alkalies, salts, moisture, and fungus, it is very hard and brittle. Consequently plasticizers and plasticizing resins must be added to make useful coatings. To make chemical- and corrosion-resistant coatings, the modifiers must like wise be nonreactive with acids, alkalies, and salts. As little as five per cent of a saponifiable material, such as linseed oil, alkyd resin, or ester plasticizer, seriously detracts from the alkali resistance of the finished coating. Monsanto Aroclor compounds, such as Aroclor 5460 and Aroclor 1254 or 1260, are the best available plasticizing resin and plasticizers, respectively, since they are unaffected by acids, alkalies, or salts. The following formulations illustrate the use of Aroclor compounds in combination with chlorinated rubber to make chemically re sistant maintenance coatings: ' 31 SVV 321997 STLCOPCB4073647 Ingradianfs Primers 93* 94k _________________Top Cn*1i 95 96 Paris by Waight 97 Parlon* (20-cp) chlorinated rubber Long-oil drying alkyd Akoclor. 1254 Aroclor 5460 Dioctyl Sebacate Titanium Dioxide Zinc Oxide Zinc Dust Silica Flour Carbon Black Red Lead (97%) Eipchlorohydrin Dibasic Lead Phosphite Bentone** 34 gelling agent Xylene Solvesso 140 Solt'esso 150 Turpentine Amsco***D too 44 27 . ^,, _m m__ 555 0.6 4 12 104 __ 33 280 100 __ 43 27 -- 1015 __ _ 0.45 4 12 we75 __ 25 200 100 54.5 27 __ 116 ___ ---- __ ' 1.2 ww 0.5 4 12 79 __ 21 200 100 ---- 43.5 27 11 116 ` __ 1.2 0.5 4 12 WW - ' 79 ww 21 200 100 ww 55.5 33 __ 89 11 3 ' __ 12 __ 237 26 a) Good adhesion to steel; resists salt-fog test or water immersion at 100'F b) Outstanding resistance to salt-fog test or water immersion at 100F c) Meets alkali-resistance requirements of Federal Specification TT-P-91 <t) For basement floors 98* 100 44.5 55.5 89 11 16.5 1 12 239 __ ' r.. The high-alkali content of fresh concrete or masonry requires the use of saponification-resistant modifying resins and plasticizers in chlorinated-rubber coatings. In highway paints, the need for corrosive-resistant plasticizers is further intensified by the spreading of salt and other chemi cals during winter. The abrasive action of sand, cinders, etc. on highway markings requires the use of nonoxidizing materials that do not harden and cause embrittlement and loss of abra sion resistance of the paint. The alkali- and chemical-resistant and nonoxidizing Aroclor compounds meet the stringent requirements for highway-paint plasticizers. Swimming-pool paints modified only with Aroclor plasticizers are much more resistant to blistering than chlorinated-rubber paints modified with alkyd resins. High pigment-volume con centration is recommended for concrete swimming pools to let the moisture in the concrete above the water line escape without buildup of blister-causing hydrostatic pressure. Low pig ment-volume concentration is suggested for steel swimming pools, however, to help form a water-impervious film to reduce blistering. The following suggested swimming-pool-paint for mulations have given excellent performance: 9 Tndeowrk of Hercules Powder Company 99 Trademark of National Lead Company 999 Trademark of American Mineral Spirits Company 32 DSW 321998 STLCOPCB4073648 I `j Ingredients For ConerU W 100* Parts by WiijM For Steel 101 >- Lacquer Phase Parlon (20-cp) chlorinated rubber 100 100 100 Duraplex* C-49 (100%)' Aroclor 1254 50 . 50 50 50 50 50 Titanium Dioxide (Rutile) 112 112 50.5 Magnesium Silicate 115 116 50.7 Phthalocyaninc Green 2.9 3 1.3 \ Bcntone 54 gelling agent Tween** 60 surfactant 13 * __ 12 8.5 5 \ Epichlorohydrin 1 r_ 0.6 Xylene " 450 210 285 Solvesso 100 90 50.7 28 Water Phase Methyl Cellulose (4000 cp) Sodium Oleate Distilled Water Properties 7.6 15.7 -- 520< ' --- Solids, wt. per cent Pigment volume-concentration, % Viscosity, Krebs units Viscosity, Brookfield, cp. No. 4 spindle, 30 rpm No. 4 spindle, 12 rpm 45.1 35 24 . -- 64.1 354 V 6,000 12,000 50.0 20 75 -- i a) Emulsion, prepared by slow addition of water phase to lacquer phase with mixing until smooth emulsion is formed I b) Meets gloss requirements of Federal Specification TT-P-95 . c) Compatabilized by the presence of AROCLOR 1254 d) In lacquer phase The use of Aroclor plasticizers in chlorinated-rubber coatings for railroad equipment helps im 1 prove the necessary resistance to high humidity, extreme weathering, and various chemicals and fumes. The following suggested formulations for a primer-and-topcoat system provide maximum chemical resistance, especially for use on tank, hopper, and cattle cars and on right- of-way equipment in industrialized or coastal areas: Ingredients . 102 Primer Parts by Weight 103 Topcoat Parlon (20-cp.) chlorinated rubber .__ 100 Arotdaz 1365 Ba^elite CKU-5962 phenolic resin dispersion 62 38 -- -- Maleic Acid 2-- Aroclor 1254 Aroclor 5460 .-- -- , <9 26 Titanium Dioxide __ 157 Lampblack -- 0.9 Zinc Chromate 105 ` -- Magnesium Silicate 19 -- Aluminum Stcrate (10% gel in xylene) 1.5 -- Cobalt Naphlhenatc (6% cobalt) .-- 0.08 Epichlorohydrin '-- 0.5 Epoxy Stabilizer --2 Antiskinning Agent Xylene 2-- 270 290 Hi-Flash Naphtha __ 158 Turpentine -- 79 TndtnirL of Rohm & Hiu Co. * Trademark of Atlw Powder Co. Trademark of Archrr*T)anicU*Midttrvd Co. Trademark of Unton Carbtdc Corp. . SW32l99g STLCOPCB4073649 Chlorinated rubber makes effective wood coatings for long service life, as illustrated by the following formulations: " Ingredients Porlon chlorinated rubber Long-oil dryingalkyd Duraplcx C-55 Linseed oil Aroclor 1254 Aroclor 5460 Titanium Dioxide Xylene Hi-Flash Kaphtha Sohcsso 100 Turpentine Mineral Spirits - A 104* 77 (20 cj>) 21 __ __ 2) __ 96.5 89.5 77 .__ __ -- 105* Parts by Weight 100 (20 cp) --. 50 __ 50 *__ __ 40 -- 320 40 -- 106' 100 (10 cp) --' --- 115 14 57 __ -- -- 286 -- 286 a) Marine finish with good resistance to salt water and to algae and other marine growth t>) Extremely abrasion resistant C) Rapid-drying finish. Partial replacement of linseed oil with Aroclor 5460 speeds the dry time and improves the alkali and chemical resistance. The Aroclor plasticizes the oxidized linseed oil to prevent brittleness. A three-coat, high-build, maintenance-paint system has been developed, based on an all-chlor inated vehicle: chlorinated rubber and Aroclor plasticizers. Conventional brush or spray coats are usually only about 1 mil thick, so at least five coats are needed to attain the minimum S-mil thickness recommended for maximum chemical resistance. The required thickness is easily built up with the chlorinated coatings by either brushing or spraying: primer, 2 mils; mid coat, 3 mils; and top coat, 1 mil. This new system has been compared with all classes of commercial. maintenance coatings in both laboratory and exposure tests. Coated panels were subjected to spot tests and immersion tests in salt fog and hot water with various chemical reagents. Color slides of the test panels are available for examination from Hercules Powder Company, Wilmington, Delaware. Ingredients Primer Parlon Chlorinated Rubber Aroclor 1254 Aroclor 5460 Dioctyl Sebacate Red Lead (97% grade) Zinc Yellow Mica Indian Red * Talc fientone 38 gelling agent Magnesium Silicate Titanium Dioxide (Rutile) Lampblack Stabilizer A-5 ** Epichlorohydrin Toluene Xylene 100 (20 cp.) 55 26.5 182 30 30 5 68.5 13 3 0.5 470 ... ` * C. 1C. William Co., Dsv. of Chu. Pfiicr & Co., Inc. ** Union Carbide Plaaiica Co. 34 ' Mid Coat Parts by Weight 100 (20 cp.) 49.5 24.8 ... 32 mm~ 3.3 77 20 1.6 3 0.5 518 .... Top Coat 100 (10 40 24 '. 10 sen Men ______ nn nn - 115 1.3 3 0.5 186 187 osW 32200 0 STLCOPCB4073650 A recently-developed continuous-painting process for finishing metal offers savings on capital investment, plant space, and operating costs. The technique utilizes the physical properties of trichloroethylene, the only solvent in the paint. Metal parts enter the unit covered with grease and leave the other end completely painted and dry to the touch. Detailed information about the process can be obtained from Du Pont, Wilmington, Delaware. The following formulation has given good characteristics in this continuous-painting system: Inara dients " *' Parlon chlorinated rubber (20-cp) Long-oil drying resin Aroclor 1254 Titanium Dioxide (Rutile) Bcntone 38 gelling agent Epoxy stabilizer Trichloroethylene - Vehicle 67 8 33.5 ___ 2.6 143 107 Parts by Waight Figmant Dispersion* __ 25 __ 100 1.31- _ 54 a) Add pigment dispersion to the vehicle after 24 hours in pebble mill b) Add 'gelling agent to pigment dispersion during last two hours of grind Mastic compositions are used to deposit thick films with a minimum number of coats. Mastics modified with Aroclor compounds can effectively seal cracks in concrete, smooth rough concrete surfaces for subsequent glossy coatings, give excellent corrosion resistance under se vere conditions, and retard fire. A typical starting formulation is the following: Ingredient! 103 Parts by Weight Parlon chlorinated rubber(20-cp) Aroclor 125H - . Aroclor 5460 Asbestos Titanium Dioxide (Rutile) Toluene . 100 .30 49 160 25 300 Although this mastic formulation adheres well to either wood or masonry, a primer is suggested before application to steel. To further increase fire retardance, replacement of 33 parts of the asbestos by 47 parts of antimony oxide is suggested as a starting formulation. A combination of chlorinated rubber and a rosin-derived alkyd resin, plasticized with Aroclor 1254, forms the basis of a high-gloss paper coating that is nonblocking and heat sealable. It gives a gloss of 79, is nonblocking either face-to-face or face-to-back for 40 hours at 130' F and 2 psi, and is heat sealed in % second at 275 F and 120 psi. Ingredients Parlon Chlorinated Rubber (10 cp.) J-feolyn* 23 Rosin-Derived Alkyd Resin Aroclor 1254 Toluene . Paper Coating parts by weight 47.4 52.6 5.3 105 Trademark cf Hercules Powder Co. 35 DSW 322001 STLCOPCB4073651 CHLORINATED POLYPROPYLENE Chlorinated polypropylene produces clear, colorless films, appears equal to chlorinated natural rubber in chemical resistance, and is noticeably more heat and light' stable. Aroclor plastici zers are very compatible with the resin and are recommended in the following starting formu lations: Ingredienti Chlorinated Polypropylene Aroclor. 5460 Aroclor 1254 Dioctyl Sebacate Epoxy Stabilixer Toluene - 109 Parts by Weight 100 (10 cp) 27 44 7.8 3.1 260 no too (20 cp) 27 44 7.8 3.1 260 300*F Heat Stability 1 hour 2 hours 3 houra S houra 18 houra v. si. yellow v. si. yellow si. yellow mod. yellow black Film Properties* v. si. yellow si. yellow mod. yellow _ -- Sunlight Stability* 24 hours 48 hours 96 houra 144 hours ' si. yellow si. yellow mod. yellow mod. yellow v. si. yellow si. yellow si. yellow brown Two-uiee^ Chemical Resistance ` Water 10% hydrochloric acid 1% sodium hydroxide .` excellent excellent excellent . excellent excellent excellent a) Lacquers were sprayed on "bonderixed'" steel panels. Films were 2.5- to 3.0-mils thick after hours air drying. *Dctermined in the Atlas Electric Devices Co. Fade-Ometer 36 DSW 322002 STLCOPCB4073652 STYRENE-BUTADIENE COPOLYMERS Styrene-butadiene-copolymcr resins are widely used in the following suface-coatings applica tions: Enamels Maintenance finishes Exterior masonry finishes Alumiijum finishes Wall scalers . Paper coatings Printing inks ' These resins form films by evaporation of solvent. Paint formulations based on styrene-buta diene resins have demonstrated the following advantages: II ' Good resistance to alkalies and acids i 11 ' Excellent water resistance Satisfactory rate of moisture-vapor transmission I Tough, durable films Excellent adhesion to masonry and allied surfaces Resistance to mildew Resistance to staining and discoloration Self-cleaning through controlled pigment chalking Ease of application Rapid drying Excellent can stability . The most common plasticizers for styrene-butadiene resins are the Aroclor compounds, but Santicizer B-16, Santicizer 160, dibutyl phthalate, dioctyl phthalate, and tricrcsyl phos phate are also useful. i. < 37 t i. DSW 322003 STLCOPCB4073653 .t Shown below are several example formulations based on these copolymer resins: Ingredients V III* II2<> 113* Parts by Weight Pliolite* S-3 Pliolite S-5 Pliolite S-5A Pliolite VT Aroclor 1254 ' Aroclor 5460 Titanium Dioxide (Rutile) Phthalocyanine Green Toner Lampblack Zinc Oxide Magnesium Silicate Diatomaceous Silica Mica Calcium Carbonate Soya Lecithin Thixcin** Thixotropic Agent Aluminum Stearate (di-acid) Hi-Flash Naphtha Mineral Spirits Solvesso 100 Toluene VM S' P Naphtha a) White, non-chalking stucco paint . i _97 ^-- . '__ 100 MM 48 48 242< 50 50 140 MM _, 69 278 103.5 11.6 1.2 .. - MM 87 93 320 __ 6 ---- _ , 234 308 234 308 __ ^ _ __ ' __ MM __ 100 ; ---- 48 52 160 --,, 80 144 6.4 __ 6.4 127 190 b) Green masonry and swimming-pool paint c) White traffic paint d) For chalking paint: substitute titanium dioxide (anatasc) II4<> 100 49 53 164 _. __ __ 82 __ 147 6.6 MM 6.6 __ 309 Formula 115 illustrates a wall primer-sealer: Ingredients Pliolite S-5A (33Va % in petroleumnaphtha) Aroclor 5460 (50% in mineralspirits) Aroclor 1254 Lithopone Titanium Dioxide (Rutile) Magnesium Silicate Soya Lecithin Aluminum Stearate Mineral Spirits #10 A/trr grinding in pebble mill, add the following: Pliolite S-5A (JJ'/j% in petroleum naphtha) Mineral Spirits #10 . ` a) Solids contents * Trademark of Coodrcar Tire V Rubber Co. for ityrenc-butadienc reainj Trademark of Baker Caalof Oil Co. 115 Parts by Weight 48* 22.5* 11 92 16 20 '1.6 1.6 27.5 . '52* 11.5 38 DSW 322004 STLCOPCB4073654 t J I <( i ; i The following formulations represent metal lacquers for three applications: Ingredients Marbon* "9200" LLV Marbon "9200" LV Marbon "9200" MV Aroclor 1254 Aroclor 5460 Aluminum Paste Pale Gold Brilliant**. # 137 ' Mica (water-ground to 325 mesh) SC*** 100 hydrogenated naphtha Mineral Spirits Xylene Ethanol Ethyl Acetate " lit* 100 25 . -- .. .... '.__ 12.5 112.5 Dry Time (Dust Free), min. Viscosity #4 Ford Cup, sec. 20 ' 511 'a) Clear, rapid-drying hard lacquer b) Low-cost, general-purpose, interior, aluminum enamel c) Gold-bronse, decorative finish II7> . Pads by Weigh! ... 100 - __ 81 181 116 __ 108.5 . ----455 303 __ -- 10 14 118* - __ --' 100 26 42 -- 157 --. Ill 163 -- __ -- . -- A variety of styrene-butadiene-based paints are illustrated by the following starting formulations: Ingredients i 19" Marbon 9545 chips Marbon 9548 chips Marbon 9551 chips . Marbon 9566 chips Marbon 10S29 chips Marbon "9200" MV Raw Tung Oil Aroclor 1254 Aroclor 5460 Titanium Dioxide (Anatase) Zinc Oxide Extra-Fine Talc Diatomaceous Silica Chrome Green A 4464 China Clay Lecithin Aluminum Stearate Cobalt Naphthenate (6% cobalt) Zinc Naphthenate (89b tine) AFAt X2280 Bentone #34 gelling agent Mineral Spirits (Low Odor) Hi-Flash Naphtha Petroleum naphtha 7 40 ' 43.5 9.5 __ 5.5 19 15.5 __ - ^, m i_ 0.05 0.09 0.12 133 a) Tile-red, high-gloss, concrete-floor paint b) White, exterior, masonry paint t) Flat, white, interior, wall paint d) Dark-green, gloss, trim enamel ' Trademark of Bott'Wimcr Corp. for atyrencbutadicne resin Trademark of Crescent Brcim Powder Co. Ttademttk of Central Solvents tf Cbrmicals Co. t Trademark of imperial Paper Color Corp. I20l> 121* Peris by Weigh! I22< __ __ __ 100 49.3 49.4 129 37 128 _ . r| ... 232 . __ 23.6 --- __ 72.8 . 3.6 __ __ __ 100 1.3 __ 12 28 10.5 __ 33 __ __ 10 ____ 9.9 ... .__ 88 35 0.59 0.9 0.135 .... 0.027 . __ 3 50 137.5 52 142 ---- \ 39 DSW 322005 STLCOPCB4073655 * The following formulations are suggested for a highway paint and an exterior masonry paint based on styrene-butadiene: Ingradianft v*. Piccoflex 120 (flaked) (solids) Santicizer 160 or Dibutyl Phthalate Aroclor 1260 ,, Ti-Pure** Titanium Dioxide (Rutile) Zinc Oxide Baiium Sulfate - Talc Diatomaceous silica Mica Calcium carbonate (dry ground) Aluminum Stearate Lecithin Methyl ester of partially hydrogenated wood rosin Troyifjd*** ABC drier VM and P Naphtha Hi-flash Naphtha Toluene 123* too* * 24 Parts by Weight ` lll(R-SlO) 57 __ - . 279 WHS .. m-- 5.2 3.7 1 IS 178 1243 100< ,,,, 21 122 (R41 61 --m 57 20 160 5.5 2 269 c) Traffic-lane paint: fast drying, nonbleeding on asphalt, no embrittlement with age b) Exterior masonry paint c) 60-% cold-cut solution with toluene d) 50-% cold-cut solution with hi-flash naphtha Procedure ' Grind pigments in styrene-butadiene solution and plasticizers. Add remainder of solvent (and stir diatomaceous silica into Formulation 123). SYNTHETIC RUBBER Many Monsanto plasticizers are usable in rubber-based surface coatings, although dibutyl phthalate, dioctyl phthalate, San ticizer 160, and tricresyl phosphate are most commonly used. Plasticizers improve gloss and flexibility in most cases. In crepe-rubber-paint formulations the use of Aroclor 1262 (from S- to SO-per cent of the weight of the rubber) increases the gloss, alkali resistance, and adhesivity to steel. * Tndtmuk of Pentuylvanu Industml Chemical Corp. for tyrtrte'buudicne copolymer rciinr Trademark of E. I. du Pont dc Nemours V Co. *** Trademark of Trot Chemical Co. ' 40 DSW 322006 STLCOPCB4073656 " The unmodified epoxy resin specimen burns vigorously; the epoxy rosin tost strip containing Aroclor and antimony oxide is "non-burning" in an identical Dunson- burner flame. . > OTHER RESIifcOATIKSs l MONSANTO PLASTICIZERS IN EPOXIES .' Epoxy resins generally possess the highly desirable properties of: Chemical resistance i Flexibility Toughness Adhesion Available in solid, liquid, and solution forms, they are useful in several types of surface coat ings, including the following: Chemical-resistant coatings Interior and exterior maintenance coatings i Baking finishes i Laminates Plasticizers arc not ordinarily used in epoxy resins when maximum performance is desired. Be cause of their high cost, however, epoxy resins are frequently highly filled. Here the use of small amounts of plasticizer aids flow and levelling and helps eliminate "drag". Monsanto has i evaluated many plasticizers in epoxy resins, as compiled in Table IX. Ii 41 DSW 322007 STLCOPCB4073657 o I -r I< i: _m i o t- f< .? .OC5 1ffft6ttftttttd aSu ; S i 52 MX--' <OOONi*>NO^ViOONtcO^ oor-ooooooccooooccr^cocooococo a $7 WlHiXSs- r* 0m*r<t v'0> m0,Oh<mfntNm^ovopoyo z 3 zo2 % oJ s O^OOO^O^vMriqoO oo rt * 00 P* t f* t i* rt t t rt rt V zui O V) Z </> < UOI' 2 C o 2 ua.i za < tao UMi OQ 00 <3 2 a2 O 3 O it < Q. C es a* eo 0 T9? m to v~ I I OOO o *3 in O o 0d\ , 5 o*. ; <.o5Aoc3" <c9'. OOOOOOOOOOOOOOO o0sOcoOt^'^o,OHO-'}-ooOOOHO^OrtofOofSo r*)o 2; . c c * 3 J1 -- 5 1 CO <U< 'I @ O O0*OnOnOviOoOnOv^OOO`nO`nOOOoOO'On'On oo^'Or^r^O^^>r^cor>c?\r^vO'0 oooo^ooooooSuoo CO CO CO 3 OCEoL Ed oc fiC |*- :si c9r M 3: CO CO OO pu, a. OO 0000000^to000 OOOOOOOOOOOOOOO -C , Cl : 9. jC --. 2 >s JZ ~rt i10 Ci.^ ^-. '^^O2 j: *5 W 22 C3 oZZ Cl rs jz -3-S 2 2 S s S Sc u: o Cu jz VP^> _v*__ H wNJ *Hu a. uM*tf uM#4 o toC o6x* O -J u P4 8g <2.2 . 7. % 2S -2 Z 2 Q o: e 5 OO QUcocotor^coco X< 42 n C9 B & cop mc O Gb. lO ss 00 yo C i p ^4 O O JZ S * pa s B a. * o p %> SO co 4J crt CL V CO O. -o e3 o -a? o (tf J5 4-> j$C UwO (X. > II II II II II o_ to K. OtoO a.? fc O c 8m fe CO d 5 M 8 8 <3 c A. O M 00 --O"* c4 U8V3 o 2 1I c .2 -o (4 L 11 o .2 c V )* *>, . >s 0 M h c jj O i5 9,J* M w^h 2 <S DSW 322008 STLCOPCB4073658 0 i (J The following suggested formulation for a 'nitrocellulose-epoxy lacquer can be sprayed either cold or hot (with solvent modifications). It leaves a brilliant appearance. Ingredients l/j-ttc. Nitrocellulose Solid Epoxy Resin Dibutyl Phthalatc Toluene ^. Isopropanol Methyl Isobutyl Carbinol Methyl Ethyl Ketone Methyl Isobutyl Ketone 125 F<Hi by Wiiglit 75 25 25 Paris by Volume 50 10 5 10 25 AROCLOR Compounds Of all the nonreactive plasticizers evaluated, the Aroclor compounds are the most compatible. Like epoxy resins, they impart excellent chemical and oxidation resistance and improve adhe sion. Aroclor compounds should not be used when solvent resistance is required, since they are true plasticizers and are not chemically bonded to the epoxy resin. Two major disadvantages of epoxy resins--cost and flammability--are diminished through the use of Aroclor compounds. Aroclor compounds, about one-fourth the cost of epoxy resins, permit significant reductions of raw-material costs. Furthermore, non-burning compositions may be made by the use of an Aroclor compound (15 phr) with antimony oxide (5 phr). For solventless coatings the fluid .Aroclor compounds, such as Aroclor 1248 and Aroclor 1254, are most commonly used. For solvent-containing coatings the resinous Aroclor com pounds (Aroclor 1262 and Aroclor 5460) are used alone or in combination with the liquid Aroclor materials. The value of .Aroclor plasticizers (1242 and 1260) in reducing the flammability of aminecured epoxy resins and improving flexural strength and compressive-yield strength, while only slightly affecting compressive strength and heat-distortion temperature, is illustrated by the following suggested starting formulations: Ingredients^1 Liquid Epoxy Resin (EV-200) Diethylenetriamine Aroclor 1242 Aroclor 1260 Antimony Oxide Control 100 15 _ ~ 126 100 15 _ 20 --. 127 Parts by Weight 100 15 _ 15 5 Properties Flammability Heat-Distortion Temp., *C Hardness, Rockwell "M" Flexural Strength, psi Tensile Strength, psi Compressive-Yield Strength, psi Compressive Strength, psi 0.82 iny min. 117.5 104 20,100 11,400 15,700 45,000 S.E.h l'/s" 87 105 25,800 15,000 17,250 52,900 N.B/ 92 106 22,100 9,800 16,950 58,150 a) Cured 16 hours at room temperature, then 2 hours at 100'C b) S.E. = Self extinguishing c) N.B. = Nonburning 128 100 15 20 ___ ~ S.E. 2'/s" 79.5 108 21,800 10,700 17,900 52.500 129 100 15 15 __ 5 N.B. 81.0 107 22,200 12,800 16,700 52,400 43 DSW 322009 STLCOPCB4073659 Mod-Epox Reactive diluents are added to reduce the viscosity of epoxy resins to improve handling char acteristics and to permit the use of higher filler contents. Since they react with curing agents and are higher priced than the epoxy resins, however, they generally tend to result in highercost formulations. Mod-Epox, on the other hand, is af unique epoxy modifier, which not only reduces the vis cosity of liquid epoxy resins by as much as 75 per cent but also speeds cure, maintains hard ness and other chemical and physical properties, and reduces curing-agent requirements by about one-third. Thus, since it costs much less than any epoxy resin and any other reactive modifier, and since it reduces the curing-agent requirement, its incorporation generally re sults in much lower formulation cost. Furthermore, Mod-Epox is not a skin irritant like other reactive diluents. The following formulations illustrate blush- and impact-resistant coatings; number 131 has the longer working life: Ingredients ERL* 2774 Epoxy Resin Mod-Epox Magnesium Oxide (fluffy)** Titanium Dioxide Brntone 38 gelling agent ZZL**0S03 ZZL-0814 ZZLA*-0822 Toluene .' Xylene Butanol Methyl Ethyl Ketone Working Life, minutes . . 130 too 11 0.2 22 3*4 ' 13 13 2 __ __ 2 20 Parts by Weight 131 100 11 0.2 22 3*4 19 __ 14 __ 2 2 -- 45 Epoxy troweling compounds are suggested for use in patching, repairing, and coating, where maximum film thickness and chemical resistance are desired. Such coatings are used to line brick, concrete, and metal tanks, such as plating and storage tanks, where application of con ventional coatings is impractical. A formulation for a black, polyamine-cured, epoxy-resin troweling compound is as follows: ' Ingredients Liquid Epoxy Resin Dibutyl Phthalate Mod-Epox Diatomaceous Earth Sastocel FRC silica gel Lampblack Magnesium Oxide (fluffy) Dicthylcnctriamine . 132 Peris by Weight 100 A 25 AO 12 12 1 3.9 ' . Tridcmarti of Union CarbiJe Corp. Stxh it Morton Chemical Co. grade CN*90 DSW 322010 4 STLCOPCB4073660 0 l ; ' , j i I ; I i 0 Procedure Add the silica gel to a blend of the epoxy resin and dibutyl phthalate while mixing with a high-torque mixer. Slowly add the remaining pigments, with continued agitation. Disperse the pigments with one loose pass on a 3-roll mill. Add the diclhylenetriamine to the pigmented epoxy-resin component and mix thoroughly. Apply the mixture to the surface with a trowel: (Lubricate the trowel for improved smoothness.) These materials set "in 2 to- 8 hours depending upon the thickness of the coating. ACRYLICS . All-acrylic lacquers and acrylic-modified lacquer systems have stimulated a great deal of interest because of their exceptional properties. The presence of acrylic resins in both air-dry and baked finishes generally imparts: Exceptional durability Lightfastness ' * Hardness High gloss upon polishing As would be expected, finishes with such properties were pioneered by automobile manufac turers. Acrylic resins have also been utilized in aircraft paints. The addition of acrylic resins to nitrocellulose lacquers produces high-quality, better-performing industrial finishes. Proper formulation of acrylic lacquers with suitable plasticizers (such as Santicizer 160, and especially Santicizer 261 and 262, which are less volatile at baking temperatures) imparts ex ceptional adhesion and improves durability. Shown below are three suggested all-acrylic automobile lacquers: Ingredient: Roller-Mill Grind: Lucitc* 6011 or 6012 (40% solids) Titanium Dioxide (Rutile) Lampblack Bentone 14 Cellosolve Acetate Reduce With: Lurite 6011 or 6012 Santicizer 160 Cellulose Acetate Butyrate, */i-sec. Toluene Cellosolve Acetate Methyl Ethyl Ketone Solids at Spray Viscosity, % * Trsdemitfc of the Du Pont Co. 133 4.01 6.17 0.07 -- 2.51 17.86 3.76 --- 21.85 17.88 21.85 18.75 .134 Paris by Weight 3.98 6.08 0.07 0.70 2.49 17.61 3.70. -- 23.87 17.63 21.87 - 18.48 !34 4.01 6.17 0.07 -- 2.51 11.60 3.76 10.01 21.97 17.87 21.97 18.46 45 DSW 322011 STLCOPCB4073661 The following starting formulations are examples of acrylic-modified nitrocellulose and chloric ated-rubber coatings: Ingredients Acryloid* B-72 Acry'oi'if B-82 Polyfmethyl Methacrylate) R. S. Nitrocellulose ('/a sec.) Chlorinated Rubber (20 cp) Santicizer 160 _ Dioctyl Phthalate Titanium. Dioxide (Rutile) Phthalocyanine Green Chrome Green Toluene Ethanol Celtosolve Acetate Methyl Isobutyl Ketone ' > 135* __ -- 81 19 __ 25 __ 40 __ 1 315 76 76 315 * I36fc 137* Paris by Weigh! !38c __ 69 -- 31 __ -- 25 67.5 .-- __ 347 88 88 347 62.5 -- -- 62.5 ---- __ --- 37.5 37.5 -- 25 25 -- 40 ' 40 11 __ - -- 315 315 76 76 76 76 315 315 Viscosity, # 4 Ford Cup, sec. 11 -- 11 11 a) Acrylic-modificd nitrocellulose automobile lacquer b) Acrylic-modificd nitrocellulose aircraft finish, resistant to aircraft lubricants. Use MIL-P-7962 (Aer) primer. c) Acrylic-modified chlorinated-rubber lacquer POLYAMIDES Polyamides are used increasingly in surface coatings applied to such materials as paper, waxed glassine, waterproof cellophane, and plastics. Polyamide films adhere exceptionally well to these substrates and have good flexibility. Polyamide compositions are also used in printing inks, overprint varnishes, paint vehicles, and hot-melt coatings and adhesives. For most applications the polyamides need no plasticizers since they are somewhat internally plasticized. For use in hot-melt coatings and adhesives, however, external plasticizers are necessary. Performance of various Monsanto plasticizers in polyamide resins is evaluated in Table X. ZEIN . Zein, a proteinaceous material derived from corn gluten, has diverse applications, particu larly in surface coatings. Both solvent-based and water-based solutions of zein form tough, high-gloss, grease-resistant, quick-drying films. Zein coatings have superior solution stability and, in contrast to most other protein compounds, are resistant to microbial attack. . The plasticization of zein is analogous to that of other synthetic and non-synthetic high poly mers. Both primary and secondary plasticizers are commonly employed. Examples of Mon santo primary plasticizers are as follows: Santicizer 3, 8, and 9 Santolite MHP and MS-80% . Secondary plasticizers that enhance compatibility are the following: Triphenyl Phosphate Tricresyl Phosphate Dibutyl Phthalate Dioctyl Phthalate * Trtdcmttk of Rohm V Kiu Co, for acrylic ciur mint Santicizer 160 Aroclor compounds Santicizer B-16 . . 46 DSW 322012 d. STLCOPCB4073662 z 2 z 2 z 2 z z > 55 Z 55 z z z 55 z z H Z z z z z z Z z z 1/3 Z > > 11 > v> </> CO , z CO zz zz zz Z CO > Z z CO > fc Z z CO > 55 z 1 1 1 1 11 < <% << < 1I 11 H $ < << 11 NM ` (O 11 o 11 N O*n r* 40 m 11 11 Mo M t~ K) oH fO "* v> 00 00 Ok 40 > > CO CO z z > z Z > z CO 55 z z CO Z Z Z z CO z z z CO to Z z Z z CO z z z z tt Z CO z z CO z z z z tt z to z z CO z z z Z co' 50 CO tu z CL. tu > B< tu Z CL. P* tu tu CL. IL. > tu CL. z CL. CL, Cl, tu CL. (U > tU CL. z CL, CL. g %} *V-cw QS u >.3 an II a a. *KNJ G P < CO o^r ' wHS G P C2<O D io c ty l Phthalate Tricrcsyl Phofphate 40 CQ *Wr94 w OO o40 *uM 0 WH G tuC H G *O H C7<O. P CX<O p 2< CO 8 *5 < *c fi Iiii Z v> cu 5> III ft, H 9 47 DSW 322013 STLCOPCB4073663 Shown below are three starting formulations for zein-based coatings: Ingredients Zein Hydrogenated Wood Rosin WW Rosin Oleic Acid Santicizer 8 .. Santolite MHP Santicizer B-16 Dioctyl Phthalate . Pigments (optional) Water Aq. Ammonia (28%) 91% Isopropanol or 95% Ethanol \ ' ' 139* 100 100 __ 25 20 ' __ ,, ___ 190 Hoi Parts by Weight 100 50 40 ___ __ 40 (50) 230 4|e 100 50 ___ __ __ l's __ 550 20 -- c) Spirit varnish for glossy, decorative, protective label coatings b) Grease-proof, fairly water-resistant coating (either clear or pigmented) c) Overprint coating for paper stock and colored paper, characterized by exceptional gloss and resist ance to water and dilute alcohol Decorative metallic-coating formulations that impart high gloss, flexibility, greaseproofness, and water resistance can be prepared either in organic solvents, as illustrated by the following suggested starting formulations, or in water: Ingredionts 142- 143* Parts by Weight Zein Santicizer 3 . Santicizer 8 Santoute MHP . 85% Phosphoric Acid ' Aluminum Powder (optional) Bronze Powder (optional) Alcohol-Soluble Color Toluene 91% Isopropanol or 95% Ethanol ' 100 ' 60 __ 80' (100) (200) __ 20 340 a) Lacquer with strong adhesion to glassine and cellophane b) Brilliant, glossy coating for coloring metal foils 100 50 ___ 35 __ (100) (200) __ __ 300 144b 100 ___ 70 60 2.3 __ as needed ___ 230 The following zein-based coatings represent a paper-coating formulation (No. 145) and a tile-sizing formulation (No. 146): Ingredients 145* Zein Hydrogenated Wood Rosin WW Gum Rosin HMP Ester Gum Santicizer 3 Dioctyl Phthalate Acetanilide Zinc Stearate Water Aq. Ammonia (28%) 100 ' ` __ 140 60 13 7 -- d) High-gloss, flexible, low-tack, hot-melt paper coating b) Textile sizing'to impart stiffness and body Parti by Weight .. I4&b 100 30 20 25 , 500 20 46 DSW 322014 STLCOPCB4073664 ^ (0 VARNISHES AND ALKYDS .. .. The resinous Aroclor compounds are frequently used in varnishes and alkyd-resin paints to impart durability, quick, dry-time, and water and alkali resistance. The Aroclor compounds do not oxidize, and flame-retardant formulations are produced by combinations of Aroclor compounds and antimony oxide. Aroclor 4465 and Aroclor 5460 are mojt commonly used, although Aroclor 1260 is best for flexible short-oil varnisjies. A suggested starting formula is one part oil, one part Aroclor compound, and one part of another resin. Aroclor 5460 is also useful in making varnish formulations based on phenolic or ester-gum resins. Shown below are three suggested starting formulations for flame-retardant paints: Ingredients Long-oil Alkyd Resin (609 solution) Alkali-refined linseed oil Kettle-bodied linseed oil Aroclor 1254 . Aroclor 5460 Titanium Dioxide 35# Leaded Zinc Oxide Magnesium Silicate Calcium Carbonate Antimony Oxide Barium Sulfate Red Iron Oxide Japan Drier Aluminum Stearate Cobalt Naphthenate (6% cobalt) Lead Naphthenate (24# lead) Manganese Naphthenate (6% manganese) Turpentine Mineral Spirits . 147 Semi-Gloss Interior 100 . ____ __ 40 . 69 V 36 __ 31 114 0.63 2 .7 0.31 ` __ 51 148 Exterior Parts by Weight 149 Shingle Stain too 30 __ . 76 42. 180 57 76 42 __ __ _ 9.8 .. . - __ ,__ 2 .__ ___ 27 too ___ _ 62 ___ 77 77 108 .__ 3. __ 378 SILICONES Heat-resistant aluminum coatings based on silicone resins contain Aroclor compounds as im portant ingredients. Suggested starting formulations for a. heat-resistant coating, enamel, and paint arc given below. The coating (Formulation 150) can withstand continuous service at 400 F and a maximum temperature of 800 F. The enamel (N'o. 151) resists temperatures of 900 to 1000 F in such applications as jet-engine components, exhaust manifolds, and in cinerators. The paint (Xo. 152), which meets Federal Specification TT-P-0028, has excellent resistance to a programmed heat test (including 8 hours at 1200 F) and to a salt-waterspray test (after programmed heating to 500, 600, and 900 F). 49 DSW 322015 STLCOPCB4073665 fngrcditnft Dow Corning 803 Silicone Resin (50% NV) GE Silicone Resin SR-82 (60% in xylene) GE Silicone Resin SR-112 (50% in xylene) Styrene-Butadiene (50% in xylene) Aroclor 1254 Aroclor 4465 (90% nonvolatile) 60% Aroclor Solution* AROCLOR 5460 (60% in xylene) Aluminum Paste (74% nonvolatile) Cobalt Octoate (6% cobalt) Xylene Mineral Spirits a) Composition of Aroclor Solution Ingredient Aroclor 1262 Aroclor 4465 Soluesso 100 Xylene ISO Coating 100 __ _ 151 Enamel' Parts by Weight -- 36 64 151 89.5 175 51 0.9 52 Weight Per Cent 24' 36 24 16 152 Paint 15.7 84 19.5 38 97.5 57 46 PHENOL1CS . Plasticizers are frequently used to improve the cold-punching characteristics of phenolic-resin laminates. Santicizer 160, tricrcsyl phosphate, dibutyl phthalate, HB-40, and the Aroclor compounds are frequently used. The Aroclor compounds and tricrcsyl phosphate also impart flame resistance. Diphenyl phthalate is also useful in phenolic compounds. MELAMINE - In melamine coating and laminating resins, Santicizer 9 promotes solution stability and compatibility, improves flow-out during baking or curing, and reduces pigment discoloration. The final coating has improved impact resistance, abrasion resistance, and buffability. SHELLAC . '. Santicizer 8 is an excellent plasticizer for sncllr" At a concentration of 10 per cent of the weight of shellac, it has a pronounced softening effect but does not affect adhesion. Santi cizer 9 and B-16 are also useful plasticizers, but less effective than Santicizer 8. (2 50 ... $) DSW 322016 STLCOPCB4073666 i $ Santoute MHP and Santolite MS-80% aie widely used to modify synthetic resins to give films with improved water resistance, brilliance, and adhesion to many surfaces. They are compatible with a great variety of resins. Usually they are compounded with liquid plasti cizers, such as Santicizer 160 or dibutyl phthalate, but in special cases they are used with out liquid plasticizers. The resinous Aroclor compounds, widely used as svpthpfir-rpcin pvtpndprs, impart improved adhesion, chemical and oxidation resistance, and flame retardance and usually lower the formu lation cost. Aroclor 4465, 5442, and 5460 are compatible in most synthetic resins and are soluble in the common low-cost solvents. . COATING MODIFIER A variety of significant benefits is imparted to many surface coatings systems by the addition of a small quantity (usually between 0.1 and 2.0 per cent of the resin solids) of Modaflow*, Monsanto's new, novel coating modifier. A complex polymeric material, Modaflow function ally modifies surface tension and viscosity. Among its many benefits are improvement of flow, levelling, adhesion to substrates, recoatability, and drying uniformity and reduction of "fish- eyes", brushmarks, "cratering", and poor flow-out. ANTIOXIDANTS ' Extremely small concentrations of Santonox, Santonox R, and Santowhite Powder Refined antioxidants have proved to be very effective for many synthetic resins used in protective coatings. CATALYST/CLARIFIER In the production of alkyd and polyester resins and bodied oils, the presence of triphenyl phosphite shortens the processing time and results in lighter, clearer products. The processing time for a maleic anhydride-ethylene glycol polyester resin was reduced from 95 to 80 minutes, and the color was lightened from 20-25 to 15-20 APHA by the addition of 0.5-per cent tri- pbenyl phosphite. A soya oil-pentaerythritol alkyd resin was cloudly (APHA 6.7) when pro duced without triphenyl phosphite but clear (APHA 5) in the presence of 0.5-per cent of the clarifier. Similarly, the addition of 0.5-per cent triphenyl phosphite soon after alcoholysis and the addition of maleic anhydride or fumaric acid to soya, linseed, or tall oils gives bodied oils with improved color. . * Moauiov: Mmuimo Chcniol Coaptny Trtemrk. Reciitrtcd in U.S. Pitent Office. \ DS\N 322017 STLCOPCB4073667 ODOR-MASKING AGENTS Santomask* II overcomes the disagreeable odors imparted to many protective coatings by the solvent. Highly effective even in small concentrations, the product masks the foul odor with a pleasant scent. Methyl salicylate, coumarin, and vanillin are other odor-masking agents produced by Monsanto to sweeten the odor of protective-coatings formulations. PRESERVATIVES , Monsanto's complete line of industrial preservatives includes Santobrite*, Penta (pentachlorophenol), and technical sodium benzoate, which prevent fungus attack on coatings that contain natural materials susceptible to fungus. FLATTING AND THICKENING AGENTS Santocel 62 imparts dull, semi-dull, flat, and eggshell surfaces when used in lacquers and solvent-based finishes. Santocel Z is a thickening and thixotropic agent in polyvinyl chloride plastisols. MONSANTO TECHNICAL SERVICE New plasticizer materials and new plasticizing applications are under constant development and evaluation by Monsanto, producer of the greatest volume and variety of plasticizers in the world. Supplementing this laboratory research and development work is a staff of technical specialists in plasticizer technology. This technical-consultation service is available to help protective-coatings manufacturers select the best plasticizing systems for their synthetic resins. Many coatings-formulation problems are solved through the cooperative efforts of Monsanto's plasticizer technologists working with the resins and coatings technologists of the-protectivecoatings producer. Most Monsanto plasticizers arc shipped in bulk in cither tank cars or tank trucks from six wide-spread manufacturing centers and in tank trucks within established delivery zones from six more strategically located bulk-storage stations. As producer of more kinds of plasticizers than anyone else in the world (more than SO!) Monsanto offers added savings through mixed shipments of different plasticizers (compartmentcd tank cars and tank trucks or mixed truck ' lots of drums) for all of your plasticizer needs. ' * Samtouask and $amtob.itb: Monsanto Chemical Company Trademarks. Registered in U.S. Patent Office. 52 DSW 322018 STLCOPCB4073668 4 No shipping limitations apply to any Monsanto plasticizer. Shipping classifications and net contents of standard containers for the products mentioned in this bulletin arc tabulated below: Product Classification Standard Containers (net weight, lb.) 8-gal. cans 55-gal. drums Dimethyl phthalate Dibutyl phthalate Dioctyl phthalate Diisodecyl phthalate Dicyclohexyl phthalate Diphenyl phthalate Sakticizer 160 Sakticizer 165 Sakticizer 215 - Dimethyl phthalate Dibutyl phthalate Dioctyl phthalate Resin plasticizer " Resin plasticizer Resin plasticizer Butyl benzyl phthalate (Resin plasticizer) Resin plasticizer Resin plasticizer 40 40 40 ... ' ' -- 40 40 40 550 475 445 440 350 400 500 445 450 Dioctyl adipate Diisodecyl adipate Sakticizer 409 Triphenyl phosphate Tricresyl phosphate Sakticizer 140 Sakticizer 141 Resin plasticizer Resin plasticizer Resin plasticizer Resin plasticizer Resin plasticizer Resin plasticizer Resin plasticizer 40 420 40 415 45 450 __ 225" 45 520 50 545 45 495 Sakticizer M-17 Sakticizer E-15 Santicjzer B-16 Sakticizer 1-H Sakticizer 3 Sakticizer 8 Sakticizer 9 Saktolite MHP Saktolite MS-809 Saktomask 11 Santokox Saktowhite Power Refined Aroclor 1221 Aroclor 1242, 1248, 1254, 1260, 1262 Aroclor 4465 Aroclor 5460 (ilaked) HB-40 Mod-Epox Triphenyl Phosphite Resin plasticizer Resin plasticizer Resin plasticizer Resin plasticizer Resin plasticizer Resin plasticizer Resin plasticizer Synthetic resin Synthetic resin Chemical, NOIBN Chemical, NOIBN Chemical, NOIBN Synthetic resin Synthetic resins Synthetic resin Synthetic resin Resin plasticizer Chemical, NOIBN Resin plasticizer 50 45 40 ___ . 45 60fc 45 45 - ___ -- . 50 50 ' 50 -- 40 45 45 550 525 500 380" 400 530 250" ___ 540 250" 150" 150" 520 600 500 100< 450 510 500 a) Fiber drum b) 7-gallon can c) 55-gallon drum \ (9 DSW 322019 STLCOPCB4073669 TECHNICAL LITEJim'KE AEG-fT f.'ONSAuTQ fusncu^s - . . - -- --.-jOJkll The following technical bulletins and brochures give technical information about the properties and applications of the Monsanto plasticizers and other products, that are mentioned in this bulletin. Monsanto technical literature is continuously revised to contain the most recent and reliable information possible. Your request for any literature will be promptly and cheerfully filled--without obligation, of course. TitU ' Phthalate Plasticizers Diethyl Phthalate and Dimethyl Phthalate Dibutyl Phthalate ' Di-(I-ethylhexyl) Phthalate (DOP) Diisodecyl Phthalate Dicyclohexyl Phthalate Diphenyl Phthalate Santicizer 16S Santicizer 160 (butyl benzyl phthalate) Santicizer 213 - Adipate Plasticizers Dioctyl Adipate Diisodecyl Adipate ' Polymeric Plasticizer Santicizer 409 . Phlhnlyl Glycollate Plasticizers Santicizer M-17 (Methyl phthalate ethyl glycollate) Santicizer E-15 (Ethyl phthalate ethyl glycollate) Santicizer B-16 (Butyl phthalyl butyl glycollate) Phosphate Plasticizers Santicizer 140 Santicizer 141 Triphenyl Phosphate Tricresyl Phosphate ' ' Sulfonamide Plasticizers Santicizer 1-H Santicizer 3 Santicizer 8 Santicizer 9 . Aroclor Plasticizers Aroclor Plasticizers Other Plasticizers HB-40 (partially hydrogenated terphenyl) Mod-Epox (epoxy-resin modifier) Resin Additives Santolite MHP and Santolite MS-80% (Monsanto industrial resins) Coating Modifier Modaflow Catalyst/Clarifier Triphenyl Phosphite Preservatives and Stabilizers Santobrite and Pcnta for the preservation of paints Santonox and Santonox R, antioxidants for polyethylene Santowiiite Powder Refined Sodium Benzoate. Technical '_ . Odor-Masking Agents Santoxiask II, Odor-Control Agent "Coumarin Monsanto" "Methyl Salicylate Monsanto" "Vanillin Monsanto" Technical Bulletin No. PL-303 PL-302 PL-318 PL-300 PL-312 PL-319 PL-165 PL-160 PL-213 PL-304 PL-308 PL-409 PL-17 PL-15 PL-16 PL-140 PL-141 PL-301 PL-305 PL-l-H PL-3 PL-8 PL-9 PL-306 PL-40 PL-313 PL-320 CS-16 PL-317. PL-322 . SC-2 PL-324 Technical Data Sheet Technical Data Sheet PL-325 folder folder folder S4 2-29J2-0969-6 II no IN U.S.A. DSW 322020 v-i STLCOPCB4073670 4 Gentlemen: (date) Gentlemen: (date) For further detailed information about the use of For further detailed information about the x\u your plasticizers in protective coatings, I would your plasticizers in protective coatings, I w< appreciate copies of the following technical bullc- appreciate copies of the following teclmical hi tins: : tins: PL_ FL-_ PL- * PL-_ PL_ PL. PL_ PL_ PL_ PL_ PL. Comments_ Comments. NameTitleCompanyAddress-- City---- Stale. JZone_ NameTitleCompanyAddress__ City_____ State. -Zone- (date) Gentlemen: For further detailed information about the use of your plasticizers in protective coatings, I would appreciate copies of the following technical bulle tins: PL_ PL_ PL_ PL_ PL_ PL_ Comments. Gentlemen: (date) For further detailed information about the u your plasticizers in protective coatings, I v appreciate copies of the following technical i tins: PL_ PL_ PL_ PL_ PL_ PL_ Comments. NameTitleCompany. Address-- City------State- -Zone- NameTitleCompany. Address__ City_____ State. .Zone. DSW 322021 STLCOPCB4073671 FIRST CLASS Permit No. 3016 ST. LOUIS. M O . ; __________ '______________ ________ '______ ___________ --_________. . ______________________. _ ! FIRST CLASS P* rmi+ No. 3016 ST- L U!S. M O .0 ________ i!pp DS\N 322022 a: D* t <I Ui si c. < "* s'. Z L/l 1/1 LAI Z 3 03 oz >z- a. >ca- 5 O < ON U -l ui u LM K ao. a Oz > 5 I>Q -023O3 0 u ID ?3 o2 CO oa. O h* Z o uoi' <o0 e<0 _c 2 ^ --' | 2 -o N o J= < o z qZ H CO JO *c fO .3 O 3 < P 6 Oo"oo n\ ' iliii ill >- Z < >1 a. 3 ca a O h- CM U CO < -J u O OCL o a > -2 ^ i z0 o oK< co Ui xy > a m3O _c u Z3 o h <u0 e ^Lo3_ "Oc 3 o 3 oa. Z JB <: y o *oo tzoo O to 3 3 Cu fo 'c<0 ot Z CA oo00 O3 to [I3lif3i5lUIt;5ii1i'l]liil\ l$i5l5 >z- >1 -a<. ca Q O o < a. 4i o0 o oH< OO oa. rUi 5 UJ 3: Q- co > ZQ <>Q -23O CO o Z3 Clo.A 3 o o -Jo) H Z oU_fI <N _ O c -C NoO to O oZ rt<o--* t: o *oc3 Z 3 o 5 si 6 8 oo to ill! llll C 2 fe *Vi I I e >z< >1 a. ca N a O u CCMO < 7Ui ^a> > 1" ' J32 i oz > Q coa -n *C 0 o oh<* oCO u o H c Z_ UI JZ <N O ?o jJ -qc 2 -o o zvt O ZP to `oc c o 3O S< a3. ?O O ca 5S 2 STLCOPCB4073672