Document vVzdMGmK8EL684DmQDRrKx266

GEORGIA PACIFIC CORPORATION GYPSUM DIVISION TIGARD, OREGON January 16, TO: Mr ." M~: A . - PaTmowsM----Ghiea-go Mr. G. F. Fowler - Marietta -Mr.~ E. L. Aarsen - Pp'i-fc^aadMs-r'RT~irr~D'ix~en~~=-TxoftlaBd- Mr-y--A. -J. Petraldme -~Wtlmfcng-ten Mr-^_J, -B-^-Mo ss - -11 m-i ngtonMr----C-r--Wb--be hnert^', Tigard Tigard Lab--:V-' Enclosed please find the following Chicago, Illinois, plant formulas: C-970 C-971 C-97S READY MIX FILLER READY MIX' JOINT COMPOUND (HAND TOOLS) READY MIX. FILLER (FILLER "X") NEW NEW REVISED Please cancel the following Chicago, Illinois, plant formulas by removing them from your formula books: C-977 C-979 READY MIX JOINT COMPOUND (MACHINE TOOLS) READY MIX JOINT COMPOUND (HAND TOOLS) CANCELLED CANCELLED Please sign and return the attached tear sheet. TO: TIGARD GYPSUM LAB C-970 C-971 C-97S C-977 C-979 READY MIX FILLER READY MIX JOINT COMPOUND (HAND TOOLS) READY MIX FILLER (FILLER "X") READY MIX JOINT COMPOUND (MACHINE TOOLS) READY MIX JOINT COMPOUND (HAND TOOLS) NEW NEW REVISED CANCELLED CANCELLED SIGNED '11 -vl. WNG PLANT DATE / - 7_<.: SGP 0018076 4 GEORGIA PACIFIC CORPORATION GYPSUM DIVISION TIGARD, OREGON February 23, 1978 TO: T41r. M. A1.--Pa lnowslci-----Chicago Hr.'-fti F -F^v?1 - Marietta Mr. D. C-.--Gorki 11-----Portland Mr-. E. L.'Aaseii " Poitlaiid -Mr-. J. Van " Portland -Ms~ R~ Mr. l)."~WT Lehflert TigardTigard Lab Enclosed please find the following Chicago, Illinois, Plant Formula revisions: C-970 C-971 C-977 C-978 C-979 READY MIX FILLER READY MIX TOPPING COMPOUND (HAND TOOLS) READY MIX JOINT COMPOUND (HAND TOOLS) READY MIX FILLER IV READY MIX JOINT COMPOUND (HAND TOOLS) REVISED REVISED NEW REVISED REVISED Please sign and return the attached tear sheet. TO TIGARD GYPSUM LAB C-970 C-971 C-977 C-978 C-979 READY MIX FILLER READY MIX TOPPING COMPOUND (HAND TOOLS) READY MIX JOINT COMPOUND (HAND TOOLS) READY MIX FILLER READY MIX JOINT COMPOUND (HAND TOOLS SIGNED_ HCF 2/23/78 PLANT REVISED REVISED NEW REVISED REVISED DATE SGP 0018077 A February 15, 1978 t ffj Dated: 8/2/77 CHICAGO, ILLINOIS PLANTVFORMULA READY MIX JOINT COMPOUND C-9#? (HAND TOOLS) DESCRIPTION OF PRODUCT - White Ready Mix Joint Compound used for taping, topping and texturing. foz. s* e ss FORMULA Raw Material / Proxcel-CRL -/ Filler C-978 Elvace EP-200 Nalco 71D-5 -Acryaol-ASEV60*Wa ter Function , RM Spec Preservative Filler Adhesive 185 Defoamer 125 JhiukuuBi -157" Solvent Percent .05 .5 .1 <Sr- To'To Lbs/Batch 1.0 1950.0 136.0 (15.25 gals.) 2.0 4 iQr 1104.0 (133 gals.) 3T9T-.0** 3 /?3' o Approximately 56.5 lbs/100 lbs. of active ingredients (this may vary + 8 gallons per batch. so ** One batch yields Si + 1 five gallon pail Ready Mix joint compound at`62 lbs/pail. SPECIAL MIXING INSTRUCTIONS Blend ingredients in following order:1 2 3 4 5 6 7 1) Water 2) Elvace EP-200 3) Nalco 4) Filler C-978 5) Mix until filler is dispersed 6) Add Acrysol ASE-60 7) Mix until Ready Mix is smooth - pumping viscosity should be 480 + 20 to allow for 24 hour viscosity build of 100 pts. WORKING CONSISTENCY Specifications for Paste Refer to Plant Testing Procedure No. 32. If paste is not proper working consistency, a maximum of 5 cc water per 150 grams of paste may be added to adjust. Brabender: (580 + 20) For Machine tools add 7 gallons ^0 (400 + 20) pH Minimum - 9.0 Maximum - 9.5 WORKING PROPERTIES - Refer to Plant Testing Procedure No. 33. Compound shall be plastic, buttery working and free of any coarse, gritty or undispersed particles. Material shall be free from lumps due to incomplete mixing. HCF:jr Continued on Page 2... SGP 0018078 GEORGIA PACIFIC CORPORATION GYPSUM DIVISION TIGARD, OREGON May 2, 1978 TO: Mr. M. A. Palmowski - Chicago -Mr-. E. L. Aa-sen1 - -Portland" M-- 7 --mitt u. --4^11. JJ -- o < Tigard t . owieir^ OUi. IM11 yv LL!LlllL!L L Lab Plane trca Enclosed please find the following Chicago, and revision: C-970 READY MIX FILLER C-971 yi C-977^ READY MIX TOPPING COMPOUND READY MIX JOINT COMPOUND C-978 READY MIX FILLER C-979 READY MIX JOINT COMPOUND C-97 3' READY MIX FILLER Illinois, Plant Formula cancellations CANCELLED CANCELLED CANCELLED CANCELLED CANCELLED REVISED Please sign and return the attached tear sheet. TO: TIGARD GYPSUM LAB C-970 C-971 C-977 C-978 C-979 C-973 SIGNED HCF 5/2/78 READY MIX FILLER READY MIX TOPPING COMPOUND READY MIX JOINT COMPOUND READY MIX FILLER READY MIX JOINT COMPOUND READY MIX FILLER PLANT CANCELLED CANCELLED CANCELLED CANCELLED CANCELLED REVISED DATE <T-J -~p% SGP 0018079 February 22, 1978 Formula C-977 NEW CHICAGO, ILLINOIS PLANT FORMULA READY MIX JOINT COMPOUND C-977 (HAND TOOLS) DESCRIPTION OF PRODUCT - White Ready Mix Joint Compound used for taping, topping and texturing, For selected market trials and shipments to Grand Rapid s only. FORMULA Raw Materia . " Proxcel-CRL Filler C-9'27. 3 4 5 6 Elvace EP-200 Nalco 7ID-5 ''Water Function Preservative Filler Adhesive Defoamer Solvent RM Spec 185 125 Percent .05 93.35 6.5 .1 100.0 I3s/Batch 1.0 1 50.0 136.0 (15.25 gals 2.0 1104.0 (133 gals.) 3193.0** *Approximately 56.5 lbs/100 lbs. of active ingredients (this may vary + 8 gallons per batch. ** One batch yields 50+1 five gallon pail Ready Mix joint compound at 62 lbs/pail. SPECIAL MIXING INSTRUCTIONS - Blend ingredients in following order: 1) Water 2) Elvace EP-200 3) Nalco 4) Filler C-978 5) Mix until filler is dispersed 6) Mix until Ready Mix is smooth - pumping viscosity should be 480 + 20 to allow for 24 hour viscosity build of 100 pts. WORKING CONSISTENCY Specifications for Paste Refer to Plant Testing Procedure No. 32. If paste is not proper working consistency, a maximum of 5cc water per 150 grams of paste may be added to adjust. Brabender: (580 + 20) For Machine tools add 7 gallons ^0 (400 + 20) pH Minimum - 9.0 Maximum - 9.5 WORKING PROPERTIES - Refer to Plant Testing Procedure No. 33. Compound shall be plastic, buttery working and free of any coarse, gritty or undispersed particles. Material shall be free from lumps due to incomplete mixing. HCF:j r Continued on Page 2 ... SGP 0018080 February 22, 1978 Formula C-977 NEW BONDING PROPERTIES Specifications CRACK RESISTANCE Specifications COLOR Specifications - Refer to Plant Testing Procedure No. 35. After compound has dried, tape shall show at least 907o fiber tear when delaminated. - Refer to Plant Testing Procedure No. 37. Rating shall be 4 or better. y - White Dried compound shall match color of standard sample. HCF:jr SGP 0018081 February 22, 1978 Formula C-977 NEW CHICAGO, ILLINOIS PLANT FORMULA READY MIX JOINT COMPOUND C-977 (HAND TOOLS) DESCRIPTION OF PRODUCT - White Ready Mix Joint Compound used for taping, topping and texturing. For selected market trials and shipments to Grand Rapids only. FORMULA Raw Material Proxcel-CRL Filler C-978 Elvace EP-200 Nalco 71D-5 *Water Function Preservative Filler Adhesive Defoamer Solvent RM Spec 185 125 - Percent .05 93.35 6.5 .1 100.0 Lbs/Batch 1.0 1950.0 136.0 (15.25 gals 2.0 1104.0 (133 gals.) 3193.0** *Approximately 56.5 lbs/100 lbs. of active ingredients (this may vary + 8 gallons per batch. ** One batch yields 50+1 five gallon pail Ready Mix joint compound at 62 lbs/pail. SPECIAL MIXING INSTRUCTIONS - Blend ingredients in following order: 1) Water 2) Elvace EP-200 3) Nalco 4) Filler C-978 5) Mix until filler is dispersed 6) Mix until Ready Mix is smooth - pumping viscosity should be 480 + 20 to allow for 24 hour viscosity build of 100 pts. WORKING CONSISTENCY Specifications for Paste Refer to Plant Testing Procedure No. 32. If paste is not proper working consistency, a maximum of 5cc water per 150 grams of paste may be added to adjust. Brabender: (580 + 20) For Machine tools add 7 gallons HjO (400 + 20) pH Minimum - 9.0 Maximum - 9.5 WORKING PROPERTIES - Refer to Plant Testing Procedure No. 33. Compound shall be plastic, buttery working and free of any coarse, gritty or undispersed particles. Material shall be free from lumps due to incomplete mixing. HCF:jr Continued on Page 2 ... SGP 0018082 February 22, 1978 Formula C-977 NEW BONDING PROPERTIES Specifications CRACK RESISTANCE Specifications COLOR Specifications - Refer to Plant Testing Procedure No. 35. After compound has dried, tape shaj.1 show at least 90% fiber tear when delaminated. - Refer to Plant Testing Procedure No. 37. Rating shall be 4 or better. - White Dried compound shall match color of standard sample. HCF:jr SGP 0018083 October 21, 1970 NEW FORMULA CHICAGO, ILLINOIS PLANT FORMULA READY MIX JOINT COMPOUND C-977 (MACHINE TOOLS) DESCRIPTION OF PRODUCT: - White Ready Mix Joint Compound used for taping, topping and texturing. (Supplied on special request only.) FORMULA: Raw Material Function Percent Lbs/3a tch Water Solvent 'Nalco Anti-Foaming agent Polyvinyl Acetate Emulsion Adhesive 3enzofiex Plasticizer Filler C -978 Filler. - ' 0.1 7.0 0.4 92.5 100.0 2165.C0*(260 gals. 4.CO 280.00 16.00 3700.00 6165.00** 'Approximately 56.5 lbs/100 lbs. of active ingredients (this may vary ^ 8 gallons per batch. ''"'One batch yields 95+1 five gallon pail Ready Mix joint compound at 62 lbs/pail. NCREING CONSISTENCY: - Specifications for Paste: Lrabender: 385 + 20 Refer to Plant Testing Procedure No. 32. If paste is not proper working consistency, a maximum of 5 cc. water per 150 grams of paste may be added to adjust. PROPERTIES ications: Refer to Plant Testing Procedure No. 23. Compound shall be plastic, buttery working, and free of any coarse, gritty, or uncispersec particles. Material shall be free from lumps due to incomplete mixing. coeducations: Refer to Plant Tasting Procedure No'. 35. After compound has dried, tape shall show at least 757. fiber tear when delaminated. RESISTANCE: ooecirications: Refer to Plant Testing Procedure No. 37. There shall be no large fissure cracks in the wedge, and no cracks in the thinner half of the wedge. coeducations: White Dried compound shall match color of standard sample. -/ Denotes change in this reissue. SGP 0018084 March 6, 1974 Supersedes Formula C-977 Dated 1/15/74 CHICAGO, ILLINOIS PLANT FORMULA READY MIX JOINT COMPOUND C-977 (MACHINE TOOLS) DESCRIPTION OF PRODUCT: - White Ready Mix Joint Compound used for taping, topping, and texturing. FORMULA: Raw Material Water Nalco Polyvinyl Acetate Emulsion Preplasticizer Filler C-978 -' Function Solvent Anti-foaming agent Adhesive Filler Percent -0.1 7.0 92.9 100.0 Lbs/Batch 1104.00 (.138 gals.)* 2.00 147.00 (16.3 gals.) 1950.00 3203.00** *Approximately 56.5 lbs/100 lbs. of active ingredients (this may vary + 8 gallons per batch. -*One batch yields 97+1 five gallon pail Ready Mix joint compound at 62 Ibs/pail. WORKING CONSISTENCY: Specifications for Paste - Refer to Plant Testing Procedure No. 32. If paste is not proper working consistency,^ a maximum of 5 cc water per 150 grams of paste may be added to adjust. Brabender: 400 + 20 WORKING PROPERTIES: Specifications: BONDING PROPERTIES: Specifications: Refer to Plant Testing Procedure No. 33. Compound shall be plastic, buttery working, and free of any coarse, gritty, or undis persed particles. Material shall be'free from lumps due to incomplete mixing. Refer to Plant Testing Procedure No. 35. After compound has dried, tape shall show at least 907o fiber tear when delaminated. CRACK RESISTANCE: Specifications: Refer to Plant Testing Procedure No. 37. There shall be no large fissure cracks in the wedge, and no cracks in the thinner half of the wedge. COLOR: Specifications: White Dried compound shall match color of standard sample. -/ denotes change WNG:elz SGP 0018085 March 6, 1974 Supersedes Formula C-977 Dated 1/15/74 CHICAGO, ILLINOIS PLANT FORMULA READY MIX JOINT COMPOUND C-977 (MACHINE TOOLS) DESCRIPTION OF PRODUCT: - White Ready Mix Joint Compound used for taping, topping, and texturing. I FORMULA: Raw Material Function Percent Lbs/Batch Water Nalco Polyvinyl Acetate Emulsion Preplasticizer Filler C-978 Solvent Anti-foaming agent Adhesive Filler -0.1 7.0 92.9 10.0 1104.00 (138 gals.)* 2.00 147.00 (16.3 gals.) 1950.00 3203.00** *Approximately 56.5 lbs/100 lbs. of active ingredie:;s (this may vary + 8 gallons per batch. **0ne batch yields 97+1 five gallon pail Ready Mix joint compound at 62 lbs/pail. WORKING CONSISTENCY: Specifications for Paste - Refer to Plant Testing Procedure No. 32. If paste is not proper working consistency, a maximum of 5 cc water per 150 grams of paste may be added to adjust. Brabender: 400 + 20 WORKING PROPERTIES: Specifications: - Refer to Plant Testing Procedure No. 33. Compound shall be plastic, buttery working, and free of any coarse, gritty, or undis persed particles. Material shall be free from lumps due to incomplete mixing. -/ BONDING PROPERTIES: Specifications: - Refer to Plant Testing Procedure No. 35. After compound has dri<_d, tape shall show at least 907 fiber tear when delaminated. CRACK RESISTANCE: Specifications: Refer to Plant Testing Procedure No. 37. There shall be no large fissure cracks in the wedge, and no cracks in the thinner half of the wedge. COLOR: Specifications: White Dried compound shall match color of standard sample. -/ denotes change WNG:elz SGP 0018086 January 15, 1975 Supersedes Formula C-977 Dated 4/26/73- CHICAGO, ILLINOIS PLANT FORMULA READY MIX JOINT COMPOUND C-977 (MACHINE TOOLS) DESCRIPTION OF PRODUCT: - White Ready Mix Joint Compound used for taping, topping, and texturing FORMULA: Raw r-.terial Water Nalco Polvvinyl Acetate Emulsion P_ eplasticizer Filler C-978 *' Function Solvent Anti-foaming agent Adhesive Filler Percent .. 0.1 7.4 92.5 100.0 Lbs/Batch 1286.00 (155 gals.)* 2.00 156.00 (17.3 gals.) 1950.00 3394.00** *Apjroximately 56.5 lbs/100 lbs. of active ingredients (this may vary + 8 gallons per batch. **One batch yields 97+1 five gallon pail Ready Mix joint compound at 62 lbs/pail. WORKING CONSISTENCY: Specifications for Paste - Refer to Plant Testing Procedure No. 32. If paste is not proper working consistency^ a maximum of 5 cc water per 150 grams of paste may be added to adjust. Brabender: 400 + 20 WORKING PROPERTIES: Specifications: Refer to Plant Testing Procedure No. 33. Compound shall be plastic, buttery working, and free of any coarse, gritty, or undis persed particles. Material shall be free from lumps due to incomplete mixing. BONDING PROPERTIES: Specifications: Refer to Plant Testing Procedure No. 35. After compound has dried, tape shall show at least 75% fiber tear when delaminated. CRACK RESISTANCE: Specifications: Refer to Plant Testing Procedure No. 37. There shall be no large fissure cracks in the wedge, and no cracks in the thinner half of the wedge. COLOR: Specifications: White Dried compound shall match color of standard sample. -/ denotes change WNG:elz SGP 0018087 SGP 0018075 CHICAG O FO RM ULA #977 ASBESTOS CONTAINING PRODUCTS