Document v6B0dvqQXvBJjLdkr5x7d0KXq
[Monsanto
eROM NAME ft LOCATION
J. H. B r own Galt 1730
cc A. R. M.
hr
W. Morgan 1730 W. Bucknell B3NB W. Farrar R2E
0
TO : L. 0. Raether - B3NB
The two samples of Mocan foam X-299 (Chrysler) and X-295 (G.M.) were cut into 1/2" thick samples for the D.O.T. burn test. Five different fabrics were laminated to the samples using a common type glue (Elmers) for one set of samples and Monsanto super glue for the other. The formulation for the super glue is as follows:
Monflex 4814
50 PHR
Monflex 4500
50 PHR
XA-582
10 PHR
Sb203
4 PHR
These samples were conditioned in the C .`J . H . room for two weeks then burned scrim side down in the D.O. iff tes t.
The results of the D.O.T. test are as follows:
DOT
X-299
Fabric Laminated With
Yellow
Polyester
Cerex
Jersey
Super Glue White Jersey
Monkey Cloth
Inches Burned Rate - Inches/Min. Self Ext.
SENB
SENB
SENS
SENB
SENS
Inches Burned Rate - Inches/Min. Self Ext.
X-295
'
Fabric Laminated With Super Glue
SENB
SENB
SENB
SENB
DSW 587609 STLCOPCB4092945
2
X-299
DOT
Fabric Laminated With Elmers Glue
Yellow
White
Polyester
Cerex
Je rs ey
J e rs ey
Monkey Cloth
Inches Burned Rate - Inches/Min Self Ext.
6 2.7 No
SENB
6 3.0 No
6 2.8 No
6 2.1 No
Inches Burned Rate - Inches/Min. Self Ext.
X-295
Fabric Laminated With Elmers Glue
2 5.2 Yes
SENS
6 2.4 No
6 2.9 No
SENB
P.S
A similar experiment will be as soon as required raw mate rials are acquired.
DSW 587610 STLCOPCB4092946