Document v1MrQaZvLap9OQBD95VBRgQVq
United States Patent cisi
Russo
[in 3,764,576
[45] Oct. 9, 1973
[54] MOLDABLE POLYBUTYLENE TEREPHTHALATE COMPOSITIONS CONTAINING ACICULAR CALCIUM METASILICATE
[75] Inventor: Robert Victor Russo, Brooklyn, N.Y.
[73] Assignee: Celanese Corporation, New York, N.Y.
[22] Filed: Dec. 15, 1971
[21] Appl. No.: 210,190
[52] U.S. Cl................................ 260/40 R, 106/306 [51] Int. Cl.............................................C08g 51/04 [58] Field of Search.................. 260/40 R; 106/306;
423/331
[56] References Cited
UNITED STATES PATENTS
3,624,024 2,888,377
11/1971 Caldwell et al.......................... 260/40R 5/1959 Allen................................. 423/331 X
FOREIGN PATENTS OR APPLICATIONS
879,151 1,010,043
853,602
8/1971 Canada.................................... 260/40R 11/1965 GreatBritain.......................... 260/40R 11/1960 GreatBritain
OTHER PUBLICATIONS
Oleesky et al., "Handbook of Reinforced Plastics,"
Reinhold, (1964) page 530. P. Virtue, "Wallastonite-on Extender for Polysty rene," Plastics Technology, (March, 1961), pp. 49 & 50. A. Damusis, ed. "Sealants" (1967), p. 73.
Primary Examiner--Allan Lieberman Assistant Examiner--S. M. Person Attorney--Thomas J. Morgan et al.
[57] ABSTRACT
Filled thermoplastic compositions comprising linear crystallizable polybutylene terephthalate with an I.V. of from about 0.2 to 1.5 deciliters/gm and acicular calcium metasilicate (calcium silicate).
Articles molded from the thermoplastic compositions possess highly glossed surfaces which are retained at high temperatures; have superior arc resistance which increases with increasing silicate concentration; and are essentially warpage-free even under asymmetrically gated conditions.
The thermoplastic compositions and articles molded therefrom can advantageously contain up to about 60 weight percent based on the total molding composition of reinforcing agents, such as asbestos fibers, glass fibers, etc.
11 Claims, No Drawings
3,764,576
12
MOLDABLE POLYBUTYLENE TEREPHTHALATE reinforced polybutylene terephthalate molding resin,
COMPOSITIONS CONTAINING ACICULAR
with an intrinsic viscosity range of from about 0.2 to
CALCIUM METASILICATE
about 1.5 deciliters per gram having significantly im
BACKGROUND OF THE INVENTION
proved arc resistance. 5 It is also an object of this invention to provide a poly
1. Field of the Invention
butylene terephthalate molding mixture which realizes
This invention relates to thermoplastic linear crystal- essentially warp-free molded articles with improved
lizable polybutylene terephthalate (PBT) compositions tensile properties under asymmetrically gated condi
containing acicular calcium metasilicate so as to signifi tions.
cantly increase tensile strength yet realize essentially 10 Additionally, it is another object of this invention to
no anisotropic shrinkage in an asymmetrically gated, provide a filled polybutylene terephthalate molding
molded article. Reinforcing agents, such as glass fibers, can be ad
vantageously included in such compositions.
mixture which not only retains a high gloss surface fin ish on articles molded therefrom at up to about 60 weight percent filler based on the total molding compo
The invention also relates to the highly glossed sur 15 sition loading but sustains this finish for extended peri
faces of molded PBT articles and the retention of same after exposure to high temperatures realizable via the calcium metasilicate addition, and to the significant im
ods of time at high temperatures i.e., about 200C. These objects are obtained by incorporating into the
unreinforced or reinforced polybutylene terephthalate
provement in the arc resistance of products molded molding resin, acicular calcium metasilicate.
therefrom; a resistance which increases with increasing 20 calcium metasilicate concentration.
DETAILED DESCRIPTION OF THE INVENTION
2. Description of the Prior Art
The molding resin of this invention is polybutylene
Recent investigations with polybutylene terephthal terephthalate. This polymer, which is one of the gen
ate molding resin (PBT) have found it to be surpris eral type described in U.S. Pat. No. 2,465,319 to Whin-
ingly superior to polyethylene terephthalate in many 25 field and Dickson, can be produced from the reaction
important processing and performance characteristics. product of terephthalic acid or a dialkyl ester of tereph-
For example, polybutylene terephthalate can be thalic acid (especially dimethyl terephthalate), and
molded and otherwise processed at lower tempera diols having 4 carbon atoms. Suitable diols include 1,4
tures, has a shorter cycle time in the mold and does not butanediol, 1,3 butanediol 1,2 butanediol, 2,3 butanerequire as does polyethylene terephthalate, the pres 30 diol and the like.
ence of a nucleating agent to induce crystallinity. Fur thermore, when a reinforcing agent is added, such as glass, polybutylene terephthalate molding resin has a
In the production of the polybutylene terephthalate polymers used in this invention, the appropriate bis (hydroxyalkyl) terephthalate is produced as the inter
higher tensile strength, lower water absorption and bet mediate. The bis(hydroxyalkyl) terephthalate can be ter creep (flexural) properties than does similarly rein 35 prepared by reacting the dialkyl ester of terephthalic
forced polyethylene terephthalate. As a direct result, acid in which the alkyl radicals can contain from one
polybutylene terephthalate molding resin, which was first disclosed along with polyethylene terephthalate in
to seven carbon atoms with about two molecular pro portions of the diols described above. It is preferred to
U.S. Pat. No. 2,465,3 19 to Whinfield and Dickson, has use higher proportions of the diol, i.e., in excess of 1.5 been found to solve processing problems long associ 40 moles of the diol per mole of the terephthalate deriva
ated with polyethylene terephthalate and believed, by tive, since by using such proportions, the initial transes
those skilled in the art, to be equally associated with all terification is caused to take place more rapidly and
polyalkylene terephthalates. Consequently, the supe completely.
rior processing requirements and physical properties of
The reaction for the esterification is conducted under
polybutylene terephthalate molding resin makes it 45 conditions of elevated temperatures and atmospheric,
more commercially desirable, with a wider area of ap subatmospheric or superatmospheric pressure. Nor
plicability than polyethylene terephthalate.
mally, the desired temperatures of the reaction can
However, one of the more serious impediments to the range from about the boiling temperature of the reac
use of the PBT molding resin has been that, because of tion mixture to as high as 275C, if desired. its inherently low heat distortion temperature and the 50 After the polymer is prepared, and if desired for a
attendant use of reinforcing agents to raise same, the given application, reinforcing agents can be intimately
arc resistance (ASTM D-495) of reinforced articles blended by either dry blending or melt blending, blend
molded therefrom, is extremely low thereby severely ing in extruders, heated rolls or types of mixers. If de
limiting the use of the reinforced resin in electrical molding applications e.g., in distributor caps for auto
55
sired, a reinforcing agent can be blended with the monomers in the polymerization reaction as long as the
mobiles. Another problem which has detracted from the use
polymerization reaction is not affected. Alternatively, a reinforcing agent can be added after polymerization
of polybutylene terephthalate as a molding resin has re and prior to extrusion. The types of reinforcing agents
sulted from the low tensile strength of the unreinforced polymer for, when reinforcing agents have been ad
60
which can be used include, among others, glass fibers (chopped or continuous rovings) asbestos fibers, cellu-
mixed to improve this property, asymmetrically gated, losic fibers, cotton fabric paper, synthetic fibers, metal
molding applications have been effectively eliminated lic fibers and the like. The amount of reinforcing agent
i.e., anisotropic shrinkage (warpage) becomes com can range from about 2 to about 60 weight percent,
mercially unacceptable. SUMMARY OF THE INVENTION
65 preferably from about 5 to about 30 weight percent based on the total molding compositions. Reinforced polybutylene terephthalate resins have
It is an object of the present invention to provide a important advantages over equivalently reinforced
3,764,576
34
polyethylene terephthalate. Compared to polyethylene terephthalate, polybutylene terephthalate can be pro
thermal decomposition and erosin. This test is not ap plicable to materials that melt or form fluid residues
cessed at much lower temperatures, at significantly which float conductive residues out of the active test
lower cycle times and with lower mold temperatures. In area thereby preventing formation of a conductive
addition, it has noticeably higher notched Izod and ten 5 path. The early stages of the test are mild and the later
sile impact, less shrinkage and lower water absorption stages are more severe - the arc occurs intermitently than does polyethylene terephthalate. Of even greater between two electrodes resting on the surface of the significance, polybutylene terephthalate with reinforc specimen in regular or inverted orientation.
ing agents alone, i.e., with no mold release or nucleat
Although the sparking time remains constant (14 sec-
ing additives, produces molded articles with smooth, 10 ond) the severity of the test is increased by increasing
uniform, highly glossed surfaces in contradistinction to the percentage of spark-time in the on-off cycle (see
the surfaces realized on articles produced from mold Table I)
ing compositions of polyethylene terephthalate and re inforcing agents, similarly without said additives. All of
TABLE I
these improved processing and physical characteristics 15 Time cycle
of the reinforced polybutylene terephthalate resins are highly desirable having direct commerical ramifica
V4 second on
I Vi seconds off VI second on
tions, when compared to equivalently reinforced poly ethylene terephthalate resin.
VC second off Vt second on % second off
More importantly though, these improvements in
Total Time Elapsed 0-60 seconds
60-120 seconds
120-180 seconds
Comment Sparking for
H of cycle
Sparking for V4 of cycle
Sparking for W of cycle
processability and physical characteristics between
The test specimen thickness is approximately 0.125
polyethylene terephthalate on the one hand and poly inches with a flat surface for testing.
butylene terephthalate on the other hand are so dispro
It has been found that the addition of acicular cal
portionate as to lead one to the conclusion that polybu cium metasilicate to polybutylene terephthalate mold-
tylene terephthalate is different, at least physically, 25 ing resin not only significantly raises the arc resistance
from polyethylene terphthalate. That is, the improve of articles molded therefrom relative to reinforcing
ments realized by this seemingly small change in chemi agents of the prior art but continues to increase the arc
cal structure are so out of proportion, relative to what resistance with increase in calcium metasilicate con
would be and should be expected, as to make polybu centration; a totally unexpected result in view of the
tylene terephthalate entirely distinct from and unre 3(3 lack of increase obtained by increasing the concentra
lated to polyethylene terephthalate.
tion of prior art reinforcing agents such as glass and/or
Two interrelated problems have appeared during the asbestos fibers, (see Examples II-XV) Serendipitously,
molding of polybutylene terephthalate resins, espe it is also to be noted that acicular calcium metasilicate
cially for electrical products end-use.
is able to be commerically compounded with polybutyl-
First of all, the unreinforced resin has a relatively low 35 ene terephthalate at much higher concentration levels
heat distortion temperature. The heat distortion tem than is feasible with reinforcing agents such as glass
perature (ASTM 648) is measured by immersing a 5 and/or asbestos fibers.
inch long by V4 inch wide by V* inch thick molded bar in an oil bath with a 264 psi load and increasing the
It has also been discovered that because of the acicu lar, i.e., regularly uniform, needle-like, structure of the
temperature of the oil bath at 2C/minute until a total 40 calcium metasilicate, there is imparted to the resin an
deflection of 10 mils is realized, at which time the tem increase in mechanical properties such as tensile
perature is recorded.
strength and heat distortion temperature with increase
In order to raise the heat distortion temperature to a in calcium metasilicate level, demonstrating the re
commercially acceptable level, it has been common tained reinforcing nature of the material, i.e., it is not
practice to admix with the polymer a reinforcing agent 45 ground to an irregularly shaped powder in compound
or agents such as has been previously described e.g., ing.
glass fibers, abestos fibers etc. However, use of the reinforcing agents of the prior
art in admixture with polybutylene terephthalate al though successfully increasing the heat distortion tem perature as well as other physical properties of the final molded products, such as tensile strength, etc. have, first of all, not only failed to provide a molded article of sufficiently high arc resistance to be commercially acceptable in most electrical applications but secondly,
TABLE II
Composition
PBT PBT/Calcium Metasilicate PBT/Calcium Metasilicate PBT/Asbestos Fibers PBT/Glass Fibers
Composition Percentages
100 70/30 40/60
70/30 70/30
TABLE III
Heat Distoration Temperature (F)
160 (71C) 311 (155*C) 374 (I90"C)
349 (176'C) 416 (210C)
the use of reinforcing agents per se have created a problem when, of necessity, an article must be molded via an asymmetrical gate i.e., anisotropic shrinkage causes a severe and commerically unacceptable warpage of the molded articles.
Arc resistance is found by a method (ASTM 495) in tended to differentiate among similar materials with re spect to their resistance to the action of a high voltage (1 2,500 volts), low current (10 milliamps) arc close to the surface of articles molded therefrom, intending to form a conducting path therein or causing the material to become conductive due to localized chemical or
Composition
PBT PBT/Calcium Metasilicate PBT/Calcium Metasilicate PBT/Glass Fibers PBT/Asbestos Fibers PBT/Glass Fibers/Alumina PBT/Glass Fibers/ Calcium Metasilicate
Composition Percentages Percentages
100 70/30 40/60 70/30 70/30 60/30/10
60/30/10
Tensile Strength (psi) 7,500 8,900
10,100 17,000 12,100 11.500
15.900
Thus, one would expect that when molding an asym metrically gated part from an acicular calcium metasili cate filled polybutylene terephthalate resin mixture,
3,764,576
6
anisotropic shrinkage of the part would be realized as would occur with other polybutylene terephthalate/reinforcing reinforcing agent mixtures. Surprisingly, this is not the case, for although increase in tensile and heat distortion properties are realized, warpage of
then mixed for 5 to 10 minutes and the resultant poly mer discharged and chipped in the usual manner.
This example represents the preparation of a typical polybutylene terephthlate polymer being contemplated for use in the instant invention.
asymmetrically gated parts is essentially eliminated with the use of calcium metasilicate (although the use
EXAMPLE II-XV
of as little as 5 percent of a reinforcing agent will no
Polybutylene terephthalate resin, prepared in the
ticeably restore the anisotropic shrinkage condition).
manner of Example I having an intrinsic viscosity of
The teachings of the prior art acknowledge acicular 10 0.75 dl/g is added to one-eighth inch glass fibers (OC-
calcium metasilicate to be a pigment filler and that con F-409AA); asbestos fibers (Union Carbide Calidria
centrations in resins in excess of about 10 percent by grade 144) and acicular calcium metasilicate forming
weight have the effect of reducing the surface gloss of test mixtures containing from about 10 to 50 percent
articles molded from said compositions as well as pro by total weight glass fibers (difficult to extrusion com
ducing a matte finish.
15 pound at higher levels) 10 to 30 percent by total weight
It has been discovered that amounts of calcium meta asbestos fibers (unable to extrusion compound at
silicate up to and exceeding 60 weight percent of the total composition in mixtures with PBT not only did not produce a "matte" finish on the surface of articles
higher levels); and 10 to 60 percent by total weight acicular calcium metasilicate respectively. The mix tures are individually tumble blended for 1 minute and
molded therefrom, but, to the contrary, realized sur 20 then extrusion blended by force feeding through a one
faces that were extremely smooth, glossy, and highly inch single screw extruder with a strand die.
uniform.
The temperature of the extruder and die ranges from
Furthermore, when articles molded from PBT/glass; about 500 to 510F. The strands are ground in a mill
PBT/asbestos mixtures; and/or combinations of the ing type mixer to pass through a large screen (4 mesh
same are subjected to high temperature aging condi- 25 or smaller). The individual mixes are then molded into
tions the surfaces of the articles subjected to such treat 4 inch discs with thickness of 0.125 inches and arc
ment were badly decomposed and eroded i.e., appear measurements (ASTM D-495) taken on each. The re
ing like the surface of a severly rusted iron plate. sults are as follows:
Wholly unexpectedly, when an article molded from a mixture of polybutylene terephthalate and acicular cal 30 cium metasilicate was subjected to the same condi
Polybutylene Terephthalate Composition Arc Measurements
tions; the surfaces remained smooth, glossy and highly Examples
uniform.
11
It is contemplated that the acicular calcium metasili III
cate will be intimately blended in a mixture comprising
35
IV V
polybutylene terephthalate preferably from about 2 to VI
about 75 weight percent of the total composition; the
more preferred range being from about 10 to about 65
weight percent. Reinforcing agent(s) can also be pres ent preferrably up to about 60 weight percent of the
40
VJI VIII
IX
total composition. When glass fiber addition is desired
it is preferred that the glass be present from about 5 to
Composition
PBT Glass Fibers (%) 90/10 80/20 70/30 60/30 50/50 40/60 (difficult to extrusion compound) PBT/Asbestos fibers (%) 90/10 80/20 70/30 60/40 (unable to extrusion compound) PBT/CaSiOa(%)
Arc Resistance (Seconds) 145 131 130 133 132
--
125 135 130
--
about 30 weight percent of the total composition and
when the addition of asbestos fibers is contemplated, the preferred concentration is up to about 30 weight
45
XI
XII XIII
percent; the more preferred being from 1 to about 5
XIV XV
weight percent of the total composition.
90/10 80/20
70/30 60/40 50/50 40/60
139 122 141 146 169
186
The following examples are illustrative of the desir
These examples illustrate that not only is it possible
able characteristics realized by the use of acicular cal cium metasilicate in admixture with polybutylene tere
50
to exceed the arc resistance required for most electrical molding applications (approximately 180 seconds)
phthalate resin and polybutylene terephthalate resin with the use of a naturally reinforcing calcium metasili
compositions.
cate but, in addition, the arc resistance increases with
EXAMPLE I 1,200 grams of dimethylterephthalate and 900 grams
55
increasing concentration of said metasilicate as op posed to results realized with other reinforcing materi als.
of 1,4-butanediol are mixed together along with an ap
It is also to be noted that, in addition to the afore
propriate catalyst as described in the Whinfield and mentioned, acicular calcium metasilicate is signifi
Dickson U.S. Pat. No. 2,465,319 such as zinc acetate- cantly less thixotropic than the other reinforcing mate
antimony trioxide or leadoxide-zinc oxide. The temper ature is increased to approximately 200C. when 80
60
rials tested and hence, can be commerically com pounded with PBT at substantially higher concentra
percent by weight of the methanol has been removed. tions.
Vacuum is applied and the temperature is raised to 240-250C. When the intrinsic viscosity has reached
EXAMPLES XVI - XX
0.65 to 0.70 dl/g,(8 percent concentration inortho chloro phenol at 25C) vacuum is broken and 90 grams
65
The resin compositions of Example IV; IX; and XII, i.e., a PBT/30 percent by wt. glass fiber mixture;
of tetrabromophthalic anhydride and 40 grams anti PBT/30 percent by wt asbestos fiber mixture; and
mony trioxide are added under nitrogen. The mass is PBT/30 percent by wt acicular calcium metasilicate
3,764,576
78
mixture respectively are utilized to mold an asymmetri cally gated, distributor-cap under identical processing conditions. The glass and the asbestos compositions
sustain smooth, glossy and highly uniform surfaces on articles molded therefrom (a molding phenomenon) but serendipitously, retain these highly desirable sur
produce severly warped finished articles whereas any face finishes under severe high temperature aging con
distortion realized with the calcium metasilicate com 5 ditions (a thermal stabilization phenomenon).
positions is well within commercially acceptable stan dards.
EXAMPLE XXVII
A 50/45/5 percent by wt PBT/calcium metasilicate/-
Tetrabromophthalic anhydride and antimony triox
glass fiber mixture was blended in the manner of Exam ide (6.5 and 3 percent based on the weight of polybu
ples II through XV and utilized in the asymmetrically 10 tylene terephthalate) is added to the monomer mixture
gated distributor-cap mold as described above. The fin of Example 1 and the polymerization conducted in the
ished product has a noticeable warpage.
manner of said example. Glass fibers and acicular cal
The above examples illustrate that while material ad cium silicate, 30 weight percent and 10 weight percent
ditives of a reinforcing nature inherently cause aniso of the total composition respectively are tumble
tropic shrinkage in articles produced in an asymmetri 15 blended for 1 minute and then extrusion blended by
cally gated mold, the use of acicular calcium metasili force feeding through a 1 inch single screw extruder
cate simultaneously realizes the mechanical property with a strand die. The temperatures of the extruder and
advantages of a reinforcing agent while essentially die ranged from 500 to 510F. The strands were
eliminating the normally attendant article warpage.
ground in a milling type mixer to pass through a large
Conversely, it is also noted that while any substitu 20 screen (4 mesh or smaller). Specimen bars (6 inches in tion of reinforcing agents such as glass fibers, asbestos length by V4 inch in width by 1/8 inch thickness)
fibers, by calcium metasilicate will reduce the severity molded from this composition exhibit significantly im
of the orientation-induced warpage problem, as little as proved flame retardant properties.
5 percent of said reinforcing agents is sufficient quan
Therefore it is also recognized that flame retardants
tity to assure its presence.
25 may also be incorporated into the polymer composi
EXAMPLE XXI
tions of the instant invention, the more preferred being
a mixture of aromatic halides in conjunction with a
The polybutylene terephthalate polymer of Example group Vb (as taken from the Periodic Table of Ele
I is compounded with 60 weight percent of the total ments found in Advanced Inorganic Chemistry by Cot
composition of acicular calcium metasilicate and 4 30 ton and Wilkerson, Intersceince Publishers, 1962) met
inch discs molded therefrom in the manner of Exam al-containing compound as more fully described in U.S.
ples 1I-XV. The surfaces of the discs are smooth, glossy Pat. Application Ser. No. 46,823 which is incorporated
and highly uniform; not unlike discs made from unfilled herein by reference.
resin. Thus, a matte finish is not realized with PBT resin
Other additives for appearance and property im
mixtures in excess of 10 percent calcium metasilicate 35 provements can be incorporated into the molding resin
as would be expected from the teachings of the prior compositions of this invention such as colorants, plasti
art. cizers, stabilizers, hardeners and the like.
EXAMPLES XXII-XXVI
In summary, it has been discovered that the incorpo
The polymer of Example I is compounded with vari ous weight percents of the total composition of acicular calcium metasilicate; glass fibers (OCF-409); asbestos fibers; and mixtures thereof in the manner of Examples II-XV. ASTM Type 1 tensile specimens (described in D638) are molded from these compositions and placed in a circulating air oven at 200C for 100 hours. The re sults are as follows:
40 45
ration of acicular calcium metasilicate in molding res ins comprising polybutylene terephthalate will (1) im prove the arc resistance with increasing concentration of metasilicate in articles molded therefrom; (2) signifi cantly reduce anisotropic shrinkage in asymmetrically gated, molded articles; and (3) not only yield smooth, glossy, highly uniform surfaces at high calcium metasil icate loadings, but will sustain these desirable finishes under high temperature aging conditions.
High Temperature Aging
As this invention may be embodied in several forms
Example XXII
PBT <Wt*)
70
Calcium Metasi licate
Glass Fibers (OCF409)
Asbestos Fibers
30
without departing from the spirit or essential character Comment 50 thereof, the present embodiments are illustrative and
not restrictive. The scope of the invention is defined by
severe surface
the appended claims rather than by the descriptions preceding them and all embodiments which fall within
XXIII
70
30
erosion Severe surface
55
the meaning and range of equivalency of the claims are, therefore, intended to be embraced by those claims.
XXIV
70
30
erosion no erosion;
smooth,
What is claimed is: 1. A molding resin having improved arc resistance
glossy comprising an intimate blend of polybutylene tere
XXV
60
30
10
no erosion; smooth
60
phthalate having an intrinsic from about 0.2 to about 1.5
viscosity in the range of deciliters per gram, and
glossy surface
acicular calcium metasilicate present in the range of
XXVI
60
30
5
5 no erosion; from about 2 to about 75 weight percent of the total
smooth glossy
composition.
surface 65 2. The molding resin of claim 1 wherein the acicular
calcium metasilicate is present in the range of from
The above examples illustrate that not only does high about 10 to about 65 weight percent of total composi
loadings of acicular calcium metasilicate in PBT resin tion.
3,764,576
9 10
3. A molding resin having improved arc resistance in the range of from about 0.2 to about 1.5 deciliters
comprising an intimate blend of polybutylene tere- per gram; a glass fiber reinforcing agent up to about 60
phthalate having an intrinsic viscosity in the range of weight percent of the total composition; asbestos fiber
from about 0.2 to about 1.5 deciliters per gram; rein reinforcing agent up to about 30 weight percent of the
forcing agent; and acicular calcium metasilicate pres- 5 total composition; and acicular calcium metasilicate at
ent in the range of from about 2 to about 75 weight per from about 2 to about 75 weight percent of the total
cent of the total composition.
composition.
4. The molding resin of claim 3 wherein reinforcing
9. A process for preparing a molding resin having im
agent is present in the range of from about 2 to about proved arc resistance comprising intimately blending
60 weight percent of the total composition.
10 polybutylene terephthalate having an intrinsic viscosity
5. A molding resin having improved arc resistance in the range of from about 0.2 to about 1.5 deciliters
comprising an intimate blend of polybutylene tere- per gram; a glass fiber reinforcing agent at from about
phthalate having an intrinsic viscosity in the range of 5 to about 30 weight percent of the total composition;
from about 0.2 to about 1.5 deciliters per gram; glass asbestos fiber reinforcing agent at from about 1 to
fiber reinforcing agent up to about 60 weight percent 15 about 5 weight percent of the total composition;
of the total composition; asbestos fiber reinforcing agent up to about 30 weight percent of the total com position; and acicular calcium metasilicate at from about 2 to about 75 weight percent of the total compo sition.
6. A molding resin having improved arc resistance comprising an intimate blend of polybutylene tere-
20
and acicular calcium metasilicate at from about 10 to about 65 weight percent of the total composition.
10. The molding resin of claim 1 comprising in addi tion, an aromatic halide stable at temperature neces sary for melt processing polybutylene terephthalate and capable of decomposing at combustion tempera
phthalate having an intrinsic viscosity in the range of tures of polybutylene terephthalate and a group Vb
from about 0.2 to about 1.5 deciliters per gram; glass metal containing compound, wherein the weight ratio
fiber reinforcing agent at from about 5 to about 30 25 of available halide in the aromatic halide to the avail
weight percent of the total composition; asbestos fiber able group Vb metal in the group Vb metal containing
reinforcing agent at from about 1 to about 5 weight compound ranges from 0.3 to about 4.
percent of the total composition, and acicular calcium
11. The molding resin of claim 12 comprising from
metasilicate at from about 10 to about 65 weight per about 3.3 to about 16.6 weight percent halide, based on
cent of the total composition.
30 the weight of the resin of an aromatic halide selected
7. A process for preparing a molding resin having im from the group consisting of tetrabromophthalic anhy
proved arc resistance comprising intimately blending dride, tetrachlorophthalic anhydride, deca-
polybutylene terephthalate having an intrinsic viscosity bromobiphenyl ether and decachlorobiphenyl ether
in the range of from about 0.2 to about 1.5 deciliters and from about 0.7 to about 10.0 weight percent metal,
per gram with from about 10 to 65 weight percent of 35 based on the weight of the resin, of antimony trioxide,
the total composition of acicular calcium metasilicate. the ratio of available halide in the aromatic halide to
8. A process for preparing a molding resin having im available antimony in the antimony being greater than
proved arc resistance comprising intimately blending polybutylene terephthalate having an intrinsic viscosity
about 0.46 to about 4.0.
*****
45 50 55 60 65