Document rxbErrZaqnmLZOMab9oa17ygJ
H. K. PORTER COMPANY, INC
CHARLOTTE, NORTH CAROLINA
PROJECT REPORT NO. 70-03-002
DATE___________ March 6. 1970
ISSUE NO.
1 ______
TITLE: Test Procedure for Lint-Free Asbestos Products
FOR: U. S. Navy - Naval Ships Engineering Center
REQUESTED EY: Management
PURPOSE:
|jpTo develope an effective method of testing lint controlled asbestos products
vs non-treated asbestos products with the purpose of rewriting Military
!CS:5*
Specification -MIL-h66E to include lint controlled products.
SUMMARY
Test results show a large decrease in airborne dust particles when our lint free treatments are used.
The tests were performed using a special vibrator machine similar to the one described
in Military Specification MIL-1-15091C. Dust counts were made using the Midgei^.
Impinger Method.
--
Twenty and/or thirty minute tests were run on treated and untreated samples of Styles AG-110 Underwriters grade and 2225 AAA grade cloths. Lint-free Portersite was also tested against untreated woven Portersite. Lint-free products showed the following reduction in dust particles as compared to the corresponding untreated samples:
1. Twenty minute test:
1.1 Style 2225 AAA----------------------------------------------------752 1.2 Style AG-110--------------------------------------------------------872
2. Thirty minute test:
2.1 Style 2225 AAA----------------------------------------------------h3%
2.2 Style AG-110--------------------------------------------------------502
3. Thirty minute test:
3.1 Knitted' Portersite----------------------------------------692
These tests indicate that this method may be used successfully to demonstrate the effectiveness of lint-free treatments.
CONTENTS: Summary, Discussion, Conclusion, Appendix
APPROVED BY
J. W. Echerd
cc: Messrs. IT. W. Swlr
REPORTED BY
T P w--
G. R. Gilchrist
l . .j
APPENDIX
1. Twenty (20) Minute Test:
STYLE
2225 AAA ` AG-110 Und. 2225 AAA AG-110 Und.
SAMPLE SIZE INCHES
11.75 x 12 11.75 x 12 11.75 x 12 11.75 x 12
2. Thirty (30) Minute Test;
STYLE
2225 AAA AG-110 Und. 2225 AAA AG-110 Und.
SAMPLE SIZE INCHES
11.75 x 16 11.75 x 16 11.75 x 16 11.75 x 16
3. Thirty (50) Minute Test (Portersite) :
STYLE
Knitted ubven
SAMPLE SIZE INCHES
11.75 x 12 11.75 x 12
TREATMENT L.F. L.F. .
Untreated Untreated
TREATMENT L.F. L.F.
Untreated Untreated
TREATMENT L.F.
Untreated
MPCF 0.096 0.087 0.75 0.35
MPCF 0.83 0.77 1.46 1.35
MPCF 0.20 0.64
DISCUSSION
Preliminary tests involved the evaluation of several methods of shaking and striking the test samples with the percent loss calculated from sample weights. Since no two people would perform this type of physical tests identically, it was apparent that a mechanical vibrator would be necessary in order to duplicate results. Initial tests also indicated the''dust-counts" would be the preferred method to determine the effectiveness of the treated asbestos products.
The machine usetl for this/test rs a modricatranEs& tte cam described for the- vibration test in Military Specifirrstrixtri-L-509-1C - Insulation Felt, Thermal, Asbestos Fiber. The samples tested: sere vibrated at 700 vibrations per minute at a movement of one-half (5g) imrfr in an enclosed box. The Midget Impinger method was used for dust counts,'with the Impinger mounted inside the box which has an area of eight (8) cubic feet.
N
Initial tests were run on treated and untreated samples of styles AG-110 underwriters grade and 2225 AAA gaeade- cloths for twenty (20) minutes. The tests were repeated on the same styles of cloth, using larger samples, for a period of thirty (30) minutes in order to obtain higher dust counts. Samples of both woven and knitted Portersite were also tested. Results of these tests are listed in the appendix.
CONCLUSION
Comparative results of the tests indicates that the lint-free treatment tends to lose some of its effectiveness as a dust control when the testing time is increased.
This proposed test method appears adequate for determination of the effect iveness of lint-free treatments on asbestos products.