Document rRLvqwo709zL1ybkjO9eqpZa

FITa: note Re: Urotli'ine Coated Fabric December 171 19^9 cc; J.TJ. McClain S.L. Harris N. Reiser P.Y. Todd J.F. Flynn, Oakville M. Med"0f.;y Oakville Discussed above subject v/ith Vomer TI, Soldier, Textile Engineer, Bayer Dyestuffs & Chemical a Ltd t Pte. Claire. Bayer's interest in this field is the supply of resin systems to centers. They also have a licensing arrange ment in Europe for "Vi strain" ure th anc CO at ed f abric. The license includes use of 1 : Vi fit ram namo , wh ich Bayer promotes, and requires 'iifora atio J i by the covtpr 'to fabric and coating specs main.tain the quality stand.arc ablin hod ky B to -f Vis tram Thero are ' no licensees in North America iince the Vi G t ra rn name has not boon promoted and has no particular value here. Resiiitex in Barcelona is a licensee of Bayer and is supplying SEAT operations in Spain. i`s7Q cesses Tv:o processes are used in making urethane coated, fabric - direct application to fabric and transfer method. Yj strata is produced by direct application, a process requiring h or 5 passes through the coating/curing .cycle. It is not recommended for the North American market because of cost of multi-pass system. The inference was left that EuropM ean manufacturers could also have trouble competitively. , \ \ \^ The transfer method is being used by all but one manu facturer in the U.S. and Canada. This process is similar to that used in the plastisol coating method for PVC. Three alternate techniqhes are used as indicated in Fig. I. ' . \ \ i g~ \ / DSW 587681 STLCOPCB4093017 2 In Method I, the coated paper is rolled up and cured 2h hrs. Subsequently the web is put through the machine again to apply adhesive and fabric. . In Method II, fabric is brought in contact with the coating while wet and then, dried. This method requires the greatest care in maintaining operating conditions. In Method III, the operations of Method I are in tandem. In all cases a 2h hr cure of the rolled up goods is required. Subsequently the coated fabric is stripped off the paper, the latter re-used several times. In configuration, the equipment of Method III is similar to General Tire's plastisol expanded vinyl corater at Toledo v/ith the exception that the latter has a third, bloving oven in series v/ith the gelling ovens. Equ i nnon t , Design ' Recommended coatcrs are the knife type -- either knife-- oveji-roll (rubber or steel) or knife-ove^N-blanket (or both, on a turret, for maximum., flexibility). Reverse roll coater not widely used. 4 Drying of urethane solution is critical, to obtain good product. Temperature requirements are modest since only necessary to drive off solvent (ethyl acetate). Initial temp should be low to prevent surface, gelling and entrapment of solvent. Recommend a 2 or 3 stage dryer, counter current bo -P fl ow, so that temperature can be separately controlled alon length of dryer and gradually raised. Speed of travel abou 15 yds per minute. ' European machinery manufacturers are recognised as being advanced in drying equipment design. Canadian textile producers for example largely use European equipment. ' A listing of companies supplying coating equipment was provided by Bayer. Copy in file. ` Coatings ' Bayer offfcr two coatings: Impranil CH - for apparel, handbag etc Imprtoiil C - for upholstery *. .. . DSW 587682 STLCOPCB4093018 -3- Impranil C produces a little harder film, and is more stable to hydrolysis under extremes of heat and humidity. These aro polyester prcpolyniars, sold in solid chips (l00>. active) which arc dissolved for use in ethyl acetate or KEX to a 30^'.solution. Bosin has a`6 months life at 70 F. Crosslinking is done by isocyanates - Imprafix TH, and accelerator,- Impxafix BF. Film formulation is; . Inpranil 30/ - 100 parts . . Imprafix TH 75^ - 5 Imprafix BF 10;o - 5 Pot life of the formulation is 6 - 8 hours. Adhesive coats ai"e produced from Impranil modified with a high boiling plasticizer eg methyl gVcc,l acetate. Impranil data sheets are on file. Urethane formulations aro pigmented and coloured pigments. Santoeel is The finished coated fabric may also VCF sealer/printer. with both opaque used for dull finish,, be lacquered Film v/pight on the finished product is in range of 3 to h o.z per yd . : Other manufacturers are also offerinJL blocked isocyanate formulations which depend on the evaporation of the blocking agent to initiate the chemical reaction. Fabrics ' All fabrics used in urethane coating are napped or brushed. Good hand of the final product requires a high density of erect fibres onto v/hich the urethane film is laid. Both brushed woven fabrics (eg sateens) and jerseys are used. Brushed nylon jersey is common. "Weight" and type dependent on product application. Only woven (stable) fabrics can be directly coated by the Vistran process. Jerseys require the transfer process. Dominion Textile produces brushed cotton fabrics. has brushed nylon knit. . Burlington > Specifications on fabrics are forthcoming from Seidler. / DSW 587683 STLCOPCB4093019 r r -4 i f* Jve3.ea.se Paper 'T S.D T,'arren is the only release paper producer being the same company siipp3.ying the plastisol YCF processors. The company has substantial process information available and a tech service laboratory v/ith a lab size coater. This v/ill be a good contact for te'clmical information. General Bayer has a pilot coating unit 20" at Union, Mev; Jersey Verona Dyestuffs. Seidler vill supply us.names of leading coaters in Europe for our reviev/ as potential, licensors. He mentioned I-Iorschu as a leader. - EHTsma i j| \ i ilj DSW 587684 STLCOPCB4093020