Document r2pRVEXggqrQEJz8R80DQMm7
-K R -70-2 PRIMROSE SHADE "KROLOR" YELLOW K Y -790-D PROGRESS REPORT B y : J . J a c k s o n 9 /1 9 /6 6 3 /6 9
4 Q
E. I, DU PONT DE NEMOURS & COMPANY
256 VANDERPOOl. STREET NEWARK, NEW JERSEY
Serial No. KN-7Q-2
Copy No.
15
RETURN TO JACKSCN LABORATORY
FILE ROOM
NEWARK PLANT PIGMENT COLOR RESEARCH REPORT PRIMROSE SHADE "KROLOR" YELLOW KY-790-D PROGRESS REPORT
Period Covered September 19, 1966 - March, 1969 (Part Time)
fil6! 211.4 DATE: 2/17/70
NJ 14071
DUP050081874
KN-70-2 1. Numerical Pile 2* Research Office Pile, Newark 211.4 3. Newark Library Pile, 211.4 4. M. Hunt/E.Gonick, Pigments, Wilmington 5. W.S.Struve 6. F.P.Ehrich/E.P.Klenke/B.H.Perkins/Newark Library 7. A.R.Hanke/E.E.Jaffe/Newark Library 8. P.J.Monahan, Newark (Vital Records) 9. N.G.Fisher, Central Research, Wilmington 10. J.Jackson 11. R.H.Wetze 1/J. P. Maurer/J.W. Minnich/W .A.West 12. M.C.Crossan, Newport Pile 13. Extra 14. Extra 15. Extra 17, Extra
NEWARK PLANT PIGMENT COLORS RESEARCH REPORT
SUBJECT: PRIMROSE SHADE "KR0L0R" YELLOW KY-790-D PROGRESS REPORT PERIOD COVERED: SEPTEMBER 19, 1966 - March, 1969 (Part Time)
DATE SUBMITTED: 12/15/69
DATE RELEASEDi 1/30/70
ABSTRACT This report summarizes attempts to produce a primrose-shade "Krolor". The product submitted after Serai~Works development was not considered adequate to compete with cadmium pigments of the same shade range*
r et ur n t o
ACKSCN LABORATORY FILE ROOM
DUP050081875
TABLE OF CONTESTS
I, INTRODUCTION .IX. SUMMARY AND CONCLUSIONS III. RECOMMENDATIONS FOR FUTURE WORK IV. PATENT STATUS
V. EXPERIMENTAL - LABORATORYSTUDIES VI. e x p e r ime n t a l d e t a il s VII. r e f e r e n c e s
Page X 12 1 1 2 2 9
DUP050081876
X. INTRODUCTION
The desirability of offering a complete line of color possibil ities in any type of pigment is obvious. Sales requested that we develop a primrose addition to the "Krolor" line.
At the same time the project was active, utility in the plas tics trade was the major objective. Sales experience with other "Krolors" indicates that broader applications would develop for a suitable product,
II, SUMMARY AND CONCLUSIONS
1. No product completely satisfactory in color, abrasion resis tance, and thermal stability was developed during these studies. All samples submitted to Sales were criticized for one or more of these properties.
2. The shortage of equipment for manufacturing chrome yellow and "Krolors"coupled with the urgent nature of other studies, re duced the priority on this work to a low level.
3. Recent price increases and shortages of cadmium yellows and contemplated increase in yellow capacity may have changed these conclusions. Such a decision would have to be made by Sales in consultation with Research and Production.
4. The problem of the variation of Y-758-D batches in their receptivity for SiOa has not been resolved and would require a solution before premises 1 and 2 could be seriously studied. As discussed in the report, this could not be tied to soluble salt content or degree of washing.
HI. RECOMMENDATIONS FOR FUTURE WORK
1. If the decision is reached to reopen this work, a SemiWorks run of the 00280 type extended with Dow's Polystyrene should be made. Products of this general type passed the Research abrasion tests but failed Chestnut Run's Banbury Mixer tests. No such exper ience was found with other "Krolors".
2. If the above is unsatisfactory, treatment of a "Krolor"like 00280 with 10% Paraplex <354 as per 1877-54P should be considered.
3. The possible development of a new primrose base in #12 Building which lends itself to the product of more thermally stable KY-790-D is worthy of consideration. Ref, 1877--39 (NC68-24 copy attached.)
IV. PATENT STATUS
In the writer's opinion, nothing of a patentable nature was developed during these studies.
DUP050081877
V. EXPERIMENTAL - LABORATORY STUDIES
The manufacture of a primrose-shade "Krolor" has not yet been resolved.
Several problems were determined to be quite serious very early in the study.
1. Greater sensitivity of the base material to pH variations than other chrome yellows or molybdate oranges making it difficult to maintain a primrose-shade "Krolor" pigment.
2. Smaller particle size material (greater surface area) probably contributes to this difficulty.
3. Widely differing results in thermal and chemical stability resulting from application of a given amount of Si02 to the pigment surface of various primrose yellow lots of Y-758-D which were con sidered to be standard in color characteristics.
4. Need for partly washed, dried, and "baked" primrose base for maximum thermal stability,
VI. EXPERIMENTAL DETAILS
A. Laboratory Studies
1. Attempts to use wet color
The beginning studies shown in NB1848-3,4,5,12 attempted to utilize wet forms of pigment rather than the conven tional dry and baked primrose yellow. The earliest studies utilized the yellow in the form of fin drum sticks (12 Bldg.) predispersed via (a) ball milling with and without surfactants such as Tamol 850 or sodium citrate, (b) homogenization in presence of Sodium silicate (N-983) followed by 20% SiOs deposition ex N-983sulfuric acid treatment and either an aluminum sulfate or calcium Staybelite coagulation.
The best results were obtained via the homogenizer route but all fell far short of a goal product. Silica coatings were poor as judged by acid and alkali sensitivity and by electron microscopy.
Experiments 1848-13, 16, 19 attempted to utilize TK-59 slurry pre-treated with sodium silicate as a base material. These were not satisfactory even when predispersed via homogenization.
B. Use of"Baked" Y-758-D
The next group of studies was based on the premise that dried and baked Y~758-D would be necessary. Y-758-D, lot 16689 (3250 lbs,/ hr.) was successfully converted to a "Krolor" via predispersion with the homogenizer (Ref, 1848-18) (See attached).
DUP050081878
-3 -
Additional studios with baked Y-758-D showed that various lots of standardized material did not respond similarly to silica coating operations for unknown reasons. Y-758-D* 12089 (std.) was also a satisfactory base (see 1832-130}. (Ref. 1848-18,21*26*29*31*32*34,
35).
We have been unsuccessful, to date# in making any non-dried and non-baked primrose yellow primrose yellow work as well as a baked
primrose as a base for "Krolor" manufacture.
The variability of the results achieved in the laboratory with different lots of Y-758-D base material were minimized by (1) pre dispersing via colloid milling and homogenization in presence of sodium silicate, and (2) controlling the pH prior to sodium silicate/ H2S04 addition at a very high level. The best method for this
appeared to reside in use of the corning type glass electrode at room temperature, (Ref. 1848* 34*5*7*8? 40*1*4; 51,2,4,6,9; 61)
C. Study of Other Variables
1. Surfactants
a. Post Slop deposition-surface treatments
Many attempts were made to improve the abrasion
resistance of KY-790-D by such treatments. The best result achieved involved 50% extensions made with a polystyrene latex - Which axe discussed in the Semi-Works section.
Treatment with 1-10% calcium Staybelite# Emery 3554D/Igepal C0630* Neofat 10, Amberols 750* 820; Paraplex <325, G54 added to slurry form of pigment prior to filtration washing drying gave rise to little
improvement (Ref. 1848-18*21*43,45* 1877-10,61)
Reslurrying a pre-dried SW's KY-790-D# followed by addition of solutions of polystyrene-Xylol, Amberol 820 - diethylene glycol, Paraplex G25, G54 - in Perclene, filtration and drying, markedly improved the base KY-790-D lot (Ref. 1877-53* 54F). This approach deserves further study. Wet addition prior to drying the KY-790-D
was not equivalent.
Attempts to tighten Up the silicate coating of KY-790-D by wet
treatment with negative and positive SiOg sols such as
lithium
polysilicates (DuPont) or Positive Sol were unsuccessful (1877-55*
$8*66).
Attempts to utilize F~, Al+3* TiO+2 as flocculants in various ways gave no substantial improvement (Ref. 1877-56,58).
Attempts to fix SiOg coating of KY-790-D with acrylic binders were unsuccessful (Ref. 1877-57).
DUP050081879
-4-
2* Surfactants in the Predispersion
Various grades of sodium silicate were tested via the homogenization route but showed no advantage over #20 WW sodium silicate* Inclusion of Na4P2C>7 as a dispersant was not satisfactory. (Ref. 1848-54,62),
3. Pulverization of the Base Color
A single attempt using fluid energy milled Y-758-D gave a superior result versus controls made from "Vortac"-milled pigment (Ref. 1848-62), This lead should be considered in the future work on this type material. Attempts to simulate this fluid energy effect by double raicropulverization of the dry color just prior to use was not as successful although some improvement was noted (Ref. 1848-65,6).
4. Bakincr of SiQp -Coated Pigment
High temperature drying of Si02-coated KY-790-D-type pigment was found to improve the thermal resistance of the "Krolor". Unfortunately, this effect was found to be reversed by long term storage in paper containers (Ref. 1848-59A# 66/ 71B).
5. Homogenization during SiOp Coating
A rehomogenization of the slurry after 50% of the Si02 deposition was made gave a slightly improved product. Continuous cycling through a high dispersion unit may be indicated (Ref. 1848-66).
6. Effect of Electrolytes on SiO? Deposition
As indicated earlier in this report# all attempts to utilize wet forms of this pigment have failed. Assuming the soluble salt level of these wet forms utilized was higher than desired# runs were made with well-washed (4500 ohm/cm2) presscake, and dried and baked color. The presscake sample and the dry color samples made in this manner were unsuitable bases for "Krolor". A study was made of the effect of addition of sodium sulfate to this type pigment base# which led to the conclusion that the Si02 coating was markedly effected by the presence of soluble salts in the system.
Reslurrying and digestion of predried and baked Y-758-D in water# followed by washing to 4500 ohm/cm2 and redrying and baking had no appreciable effect on the Si02 receptivity of the yellow. A lot (17635) which was satisfactory before washing to a higher ohm end point was equally satisfactory after rewashing in the "Krolor" process. A lot (17631) which was unexplainably unsatisfactory as a base was unchanged after this treatment.
In all cases where poor "Krolor" products result# we have ob served a peculiar pH profile.
DUP050081880
5-
pH of premix (homogenized yellow + Na silicate)
Normal 10.1-10,3
Abnormal 10.1-10.3
pH after homogenization
10-10.2
9.3-9.5
pH readjusted to
11.5
11.5 (cold)
pH after heating to 92c
9.0-9.2
8.3-8.5 (low)
pH after adding standard ratio sodium silicate/HaS04
6.0-6.5
3-5.5 (low)
The abnormal results are typical of those achieved with well-
washed presscake or predried color. Most "Krolor" made on the prim rose base followed this pH profile, i.e., good results achieved with higher pH types (Ref. 1877-1,2,5,6).
7. Nature of Precoatinq
Attempts at changing surface of Y-758-D to make more Suitable for conversion to KY-790-D included studies on
Changes in A1(083)3 to various phosphates (1848-69? 1877-41).
Pretreating with PbSiOs
(1877-48)
Pretreating with Pb++_
(1877-49)
Pretreating with Cr04^
(1877-24)
Pretreating with M0O47
(1877-7,31)
Prereduction with Sn++
(1877-40)
Pretreating with Cyme! 301 (capable
reacting with OH** groups)
(1877-50,2)
None of these approaches gave rise to improved KY-790-D.
8. Extension of "Krolor" KY-790-D
a, A study of the effect of extension of the KY-790-Dtype "Krolor" with calcium Staybelite (25-50%) was made (1877-8). Small improvement in an abrasion test (1848-58 for method) but lowered the thermal stability in a prefluxed polystyrene test (see also SW's section).
?o. Extension of KY-790-D with polystyrene latex (33-50%) improved abrasion resistance (see 1877-16-,19,20,21,22).
Semi-Works trial of this approach was unsatisfactory in chestnut Run's Banbury Mixer (See also SW section).
9. Miscellaneous Studies
Ref. 1848-58
Laboratory abrasion test not requiring two roll mill.
Ref. 1848-60,62
Study of alternatives for 20WW sodium silicate (2X and #16) .
Ref. 1877-24
50% reduction time cycle - v si. inferior results.
DUP050081881
-6-
Ref. 1877-24
Decrease homogenization pressures - v si inferior.
Ref. 1877-25
Use of NsgCOa instead of NaOH - slightly inferior.
Ref. 1877-28
Restudy of pH adjust prior to N-983 treatment in light of SW's experience. High pH better
in lab.
D. Alternative Base Materials as Substitutes for Y-758-D
Ref. 1848-6
SrCr<>4 - This light masstone, extremely weak
material was briefly studied as a base for a ''Krolor"-type pigment. The pigment as such is more stable thermally than Y-758-D, but is
extremely green and transparent* Attempts to make "Krolors" therefrom were successful from a thermal resistance standpoint, but tinctorial properties (high transparency -
poor strength) are a serious deficiency.
Ref. 1848-8 1877-35,6
Attempts to improve the opacity of Srcr* by copcoprecipitation with PbCrO* gave rise to unattractive colored (green dull) pigments. Y-493-D - Tested as is - this pigment is an inferior base material versus Y-758-D in thermal stability. "KTolors" were not made. Y-539-D - Behaved similarly to Y-493-D. Imperial's X-3148 was tested in 1877-47 as a basis for a primrose "Krolor" and found to be similar to Y-758-D types. Imperial's X-3258 - a predarkened primrose
yellow was tested (1877-65) and found to be very slightly better than X-3148 or Y-758-D as a base for "Krolor" in abrasion resistance.
1848-14,15,28/35 1877-12,3,8,20,38,39
Non-white base primrose yellow. Tests indicate that PbcOa has a very low level of thermal stability. A primrose yellow based on a nonPbCOs process was made and converted to a a
"Krolor". Findings indicated
1. Base Material very slightly more thermally
stable. 2. ''Krolor" types more thermally stable. 3. Development of a #12 Bldg, process based on
this route would be required. 4. The product was benefitted by a fluid energy
milling of the base prior to conversion to a "Krolor".
DUP050081882
-7-
Standard Process #1 - Ref. #1 1848-18A Laboratory
1. Weigh 150 gr Y-758-D (16689 - 3148 lbs./hr. - 12 Bldg.) 2. Add 20 gr. w-983 (DuPont #20 WW sodium silicate)
3. Add 1 L.HeO 4. Premix - pH at 10.0 - 10.6. 5. Homogenize at 5000 PSI - 1 pass 6. Wash out with 100 cc HaO - pH usually 9.6 - 10.2
7. Heat to 90c. 8. Record pH - 8.15. 9. Adjust to pH - 8.0. 10. Weigh and add in 4 hrs, N-983 115 gr/600 cc H20 11. Weigh and add simultaneouslyover 5 hrs. N-27 17.3 gr/800 cc HeO
12. Stir 10 min - 90C. 13. Record pH - 4.8. 14. Readjust to pH 9.0. 15. Add sodium stayhelite solution - stir 5 min.
ex 20 gr N-528 ) 5.4 gr N-7 ) Boil 10 minutes 180 cc HsO )
16. Add 8 gr. CaCla.2H20 N-20 /200 cc in 15 rain. 17. Filter - wash to 2500 ohm/cm2 18. Dry 16 hrs./180F. - Regular or high speed pulverize. 19. Yield 188 gr. pigment.
Tests Conducted in 1848-18A Types
WR66-746 - Two roll mill into polystyrene chip - Grind up chip and
mold 20 min./400oF.
20 min./600F .
vs It, vs int.
extremely It, ext. intense
1848-18A vs Y-758-D 12839 WR66-758 - Attempt sand mill in 20J. 1848-18A - Oil absorption extremely high - had to abandon (sample too
small to repeat. 1848-18B - Above type except Emery 3534D/lgepal C0630 treated vs
Y-758-D, 12839 - MT color slightly dark and red. Gloss ~ slightly inferior Tint - si red - toner basis LF. - Weatheroraeter - much superior Viscosity - v si higher
Process #2 - Ref. 1848-52C, 54c - Further study of #1 type process using cold pH adjustments and blue tip Beckman electrodes (54C used Amber electrode).
1848-52c I. Repeat steps 1, 2, 3, 4, 5, 6
7. Record pH 10.1 - Adjust to pH 11.5 with 5% NaOH. 8. Add 150 cc H20 9. Heat to 90C. 10. Weigh and add in 4 hrs. 115 gr N983/600 cc H20. II. Weigh and add in 5 hrs. simultaneously 17.3 gr H2SO-t/800 cc EfeO.
12. Stir 10 min.
DUP050081883
-8
13. Record pH 6.0. 14. Adjust to pH 9.0 (5% NaOH):
Add - Stir 2 minutes between
15. N-15 9 gr./36 cc 1$. N-3 7.5 gr,,/30 cc.
17. N-15 11 gr,/44 cc. 18. Record pH 5.4
19. Readjust to pH 5.6-5.7, Filter wash dry, etc. like Process #1
This type process became the laboratory standard except for the sub stitution of Corning Electrode 476051 type (see 1848-59A).
Semi-Works Studies KY-790-D DSN 67-3
KY-790-D, SW00204
SW-00203 (study calcium Staybelite) KY-790-D, SW-00206 (study homogeniza tion)
00211
Attempt to scale up 1848-38C (colloid mill used for predispersion). Adjust to pH 9,45 at 92C. prior to SiOa treatment - coagulate with Ala(S04)3. Result - unsatisfactory thermal resistance,
Attempt to reproduce 1848-43D (colloid mill adjust to pH 9.6 at 92c.) calcium Staybelite coagulation. Result - unsatisfactory. Attempt to reproduce 1848-44D and 45A type colloid mill and homogenize. Adjust to pH
9.45 prior to Si02 addition, coagulate with Ala(SO4)a-Emery 3554D/Igepal C0630 treat. Result inferior to laboratory control but better than 00203, 00204.
Similar to 00206 type using better control on pH meter. pH measurement at 92C. found to be extremely difficult. Quality level achieved better than 00206 but inferior to lab goal.
Because of our inability to reproduce laboratory goal quality, the following lab studies were made in an attempt to determine causes of deviation.
1877-8 - Study of contact time yellow base-sodium silicate prior to and during predispersion.
1877-10 - Prolonged stir periods. 1877-10 - Open steam vs jacketed vessel.
1877-11 - Study of agitation. 1877-15 - Materials of construction
None of these variables were found to produce significant effect effects in the laboratory.
SW-00225 - Attempt to use cold pH adjustment process and Corning electrode, Basic process Ref. 1848-52C. Contrasted to the laboratory experience, this Semi-Works run gave results inferior to those of SW-00211;and in
ferior to the laboratory pilot run 1848-60B made with same base material.
DUP050081884
--9--
SW-00239
Further study of cold pH process.Basic process like 1848-52c except as piloted in 1848-60B (same lot of prim rose yellow). In-process samples showed that SW's
process resulted in inferior product during the SiOe coat ing. That is, homogenized pigment ex the SW's homogenizer processed in the laboratory, was definitely superior to the same material finished in the same manner in the SemiWorks .
SW-00263
Study lower SW's batch size in an attempt to determine why SW's different from laboratory. pH adjustments made via technique of adding fixed amounts of 5% KaOH to eliminate question of variation in equipment, i.e.,a scale up of the lab quantities. Again in-process samples showed failure at N983/H27 additional step.
SW-002 73
Because of the unexplained differences in requirements of laboratory pH (11.5 optimum) and Semi-Works, try lower pH
adjustment after homogenization (used 10.6-10.7 instead of 11.5 optimum in laboratory). SW's results were superior to 00263, but on the defensive versus best lab types
processed in normal (11.5 pH) manner.
SW-00280
Continue study of cold pH after homogenization. Use 10.3 pH vs 11.5 laboratory. (1) SW's run best to date. (2) SW's run on defensive vs high pH lab control. (3) 5054 extension with Dow's Polystyrene latex markedly improved abrasion resistance. (See photostat attached.)
SW-0Q282
Repeat 00273 type using Na2C03 instead of NaOH for pH
adjustment and make 50% 3xtension with Dow Latex Poly
styrene. Results similar to 00280 - slightly inferior
to best laboratory types. Polystyrene extension definitely
beneficial. A sample of this material was submitted to
Chestnut Run for evaluation (JJ-LAL 1/10/68 Ref. #5,
NC-68-2 Ref, #6) but reported to be unsatisfactory. De
tails can be found in attached report.
j
ViX, REFERENCES
1. Miscellaneous product improvement studies - JJ - Dec. 13, 1966. 2. Notebook references* 1848 - 1877. 3. DSN 67-3 "Krolor" based on Y-790-D. 4. JJ - HA - Y-75B-D - #12 Bldg, base for Y-790-D "Krolor" 1/14/67
D (copy attached). 5. JJ - JAL - Y-790-D - Primrose "Krolor" Evaluation in Plastics
1/10/68 (00282-50% Polystyrene Extension)(copy attached)
6. Acknowledgement NC-68-2 2/27/68 7. NC-68-2 Work Request Report (Copy attached) 3/19/68
8. JJ - JAL - KY-790-D Primrose "Krolor" Evaluation in Plastics
7/17/68 (copy attached).
9. Acknowledgement NC-68-24 (7/19/68) 10. NC-68-24 Work Request Report (copy attached) 10/17/68 11. Series P-68806 Comparison "Krolor" and cadmium Pigments in
Plastics 10/2/68 12. Exposure Series P68808, 6/16/69 (KY-790-00282-unsatisfactory in
vinyl),
DUP050081885
10 *13. JJ-PDG - colors Based on Predarkened Chrome Yellow 4/25/69 14. JJ-RHZ TM XY-790-D - History - Chestnut Run Evaluations (copy
attached) 12/30/69
dc
DUP050081886
!;
t r.NMULA:
CODE /- rsv..:> NAME
, V*,V
/ y '" /it' (ts/ts C' "s '> ") 3
sSlt'M'J' ts{- `Cevsrr t J (>s
i/S/sisC
' (aM SO. KTW
v/^ls Co ri A///'/ dr- W A (Z C. 7?< "C *Zr:
"A* IB" LP5 OT,
MATCHtAL
//- 9;'y/rf`>
fervor yvttfi
100 %
WT.
It M. on LOT MO.
/?6lf
0AL9.
MANI.ULATtON
TMT
,': -<.1.
<frsr2
/ /tCf //>fj/
c*; //y /*/
f/y
/'7z-]>y? *
's &s t T
jWv (Aifyr, /l/rtf/ZoffT' w$&
"! tv/ J-'A
wAi'A I/Wf/jr
S* ,ar 1, . 11
f li;|
S^w-A/AV /nt/A
J jI |!
r v</- */ fkT*:
{> (o /of
s> ) At f
urevif#
'ty/f/r fsy tss, // //F>s p//;sy2~
./. , sS* j&r*/' ___ -70-3
!
*/ a /'
/Z 'T/>s CsAntet
/Zf/rff" /o
o ^
J.
/At S^;,- */* /?/
0-. { cs- y/;,'S'
C'c-Af'V, / M'r ? A 7yA' S/ZV*^
=r fcj
/ ^rrC
~t
/3V<fc '/dfi-r?.
P /' PA'
T/rtr *9 *uo;> y, A^/V?
a ; Ayy/wr
fas'
A''/'., /!/.;
/'A'A '
>5o.i> ^ /V>j '
<7
Ar^'V ^'A;f >
cc
' t'f* *' 7 // S r//C
&Mt/0
'CLsfcf S77/i P'/Si'U^
f/ |.
trVh)
'"T/l-spcS.-Af-sf
H `g&p/y yir&f*r*Jb
U/sw
> ytAoj
j>/^
tw*
. (l-J^yt^&Ly
y/A -
WATH TIME: 1*T o p a w TO: Irr cur NESTED BY: Dr NATIONS;
2n d 2n d
3r d 4t h 3r d w r it t e n BY:
Mjy3t h
3t h
I! Go a l
CHECKED BYt
Ur .
Gr o .
MADE BYi
R.P.M.
3fi/s ~ 1 ( Ck*. F"(
DUP050081887
0 ;v
.>*.
FORMULA SHEET V
4(WT'
<y^u
(f
COLOR CODE Y^fP-Q DATE
LNAME l^Pjt/?OS K&Lo/l,
ocrater T0`p`Y
PAPEO ON
Mt'S* t/gy''7&?fj-*.szfjr.cr
a?ur ...A0/?<*> 3. 7J
HATCH SIZE-MOLS.
BATCH NO. OF "K" SAMPLE
^'y/S A
B"
K-
'*>^5
<r><r ^5t
M4f3
r 4^ 4^
100% WT.
/W/
OAL,
I MANIPULATION
"t
M/e<4j ~S/ /V oPfo
CWsW&P/t-'O'tf''
S/S Sf>J
72~& ~x
<$TS/S SC >YU^
|
f/P
/>>&>
ft /,f*S '^~CSe<^6r*&
firtrf S'// * ^o f/o* </ >?///, . c*-?-? *f\
OsfsWoPfT
}
H//3s/i^-e r*r ti/Stf S'S/S r frtuS/Z. |
7f/P^ypr~ f* 7~< O &
j
U/Sfif/r s as Pi/r sA A /As
7'</>z. ;
VewfiD 7>H --/*g--
j
<?.. 1 U/<?V?A <z*r</&t0. ~ Xr^s'fiSfA
fi'p%
AS~ZZ &>u*c^PM. to*#1
"O'; Vs i' /
'6/^jj
sPrl && ff AA-O
T(pr' yf/iMSoy hlF/V/s /fya
r<T;r /V//X" - j
h/tpfa'
H 'Crr A/J -- f4zc/ 4
c? /V/jr -
f' 4^7/ W M779'
Ci/fW*JtVtuQ'
/A / /Jjr
tf*r To ?0c ~
/ 7c c>* o Th -
- f< f.r A,y #4Ar - APt/^/!/ tftAa's,*' jr/As ** ./jy.frc /fi/wS
S~7s/0
~~
_ ^^
/Ufos/f PA? &?-? 9./ Tt--ZAL
/V7 / *~* 9 P7r A). # Ck~t*y- jr7>s7 ep-77%1^
bv(; cc
P /J
~ '^
tZdPypt? ?A' ffifi 37J --T-?> -S^ cl/' c7 X <P^----`T' <^-r /See
_s /y ?u ^
(aaX'O ]
TdfiCZ zi ^t^rt^k.
]
(j -lb 0/Aetfav Pfi $'& (
rs. ,A<? /^ wu^Ms
- VC'
y
. ,&Pt>Ao
Jy t Tw UP?
S~S =3f
'. _./ *. _ PACKAGE ' GOAL YIELD
LBS PER
-Sf i"y*s //<
p a r //
-O / a / Yf`"~" /r3/~/^..)A:,y,ct
COST GROUP * SIGNATURE
. -r/l f r\. ,-f> >;rf- > 'j
DU P050081888
CC: W. J. McClure R. A. Hageman C. W, Os kins R. Gfedd
S. Struve / A, Brizzolara Jackson
MR, H. ARNOUL NEWARK, NEW JERSEY
December 14th, 1967 Newark, New jersey
Y-758-D - #12 BUILDING - BASE FOR Y-79Q-D KROLOR
We have repeatedly attempted to utilize "well washed", #12 Building production lots as a base for Y-790'-D type
KROLOR without success. Unless new information is developed, X foresee a need for utilizing two procedures for manufacturing this code:
.1. Well washed Ernery/lgepal treated for the ink trade
2 Standard quality (not well washed or organically treated) for Y-790-D.
The present program to upgrade the gloss and dispersibility of #12 Building Chrome Yellow production, will probably make
the "Krolor" type products less desireable in thermal stability,
I recommend that facilities be maintained in #12 Building
to permit future manufacture of Chrome Yellows of our presently standard types.
In other words, we must be able to Parallel wash (as well
as Series wash for the ink and paint trade), or demonstrate the
ability to reproduce the "poorer washed" quality of Parallel
washed material via Series washing. In addition, the use of
organic treating agents for Chrome Yellow KROLOR base materials
is not desireable.
^-"7 ^
.
(
Julius Jackson Research Associate
AS
C
DUP050081889
E. I, du Pont de Nemours and Company
W.F.Spengerr.an, .B. Clark,
Chestnut Run
ii ii
.H.Mattie,
Wilmington
P ,D. Graham,
R.H.Zabel,
M,Hunt/E .Goniok,
W.S.Struve/A.A.Brizzolara
R.A.Hageman/H .Arnoul
ackson (3)
Pigments Department Newark, New Jersey
January 10, 1968
J. A, LAMIET (2) CHESTNUT RUN
Y-790-D PRIMROSE "KROLOR" EVALUATION IN PLASTICS
We are submitting a sample of lot 00282 for evaluation in plastics. This product is a 5extension made with polystyrene.
We are insterested in:
1) Your opinion as to whether or not the product is adequate in thermal stability and abrasion resistance for commercial use.
2) Your assessment of the number parts^per hundred of resin,, required to be equal to or competitive with other commercials such as cadmium yellows.
A cost analysis will be prepared when pricing of this type pigment is established.
JJ:mm
DUP050081890
DISTRICT SALfcj
________TiL...
rrin-'CTorj.r.rsT. k r et t o h J!
/H
:'.;:cvfr!'i mg r .... --... J ,h. Danlet
!'.:';;v[cr jr-.w... ..
1', 3,,Reeve
....i-'iCM. c.:;. . KfilJ. 0.7
C.K._
:v i-r.ir . . . "'"CNM'.OA'. I'.'GR... .
v: P.D -Grrafoaui.
c.s. p!c-:m. WiLH.,,
R.H.Zabel, Pigm.Vilm.
\:. S.St rave./A.A,Brisz Clara, Pigm.Nwk.
r.Arnoal. P::.pn\, iT.-k.
CHESTNUT bu m SATE:.. _______
2/27/68
w ::
... - vr #2
o r-.*;.. H?:,: =j'P;:........ _............. .........._ .TTi-NTiQfv - J. JACKSOI?
................. _..... .......... ........ ................................-i-'O.:,_____________________________________________
't .t %"luate y-790vD, P.Q'i'. QQ?2, In plastics._________________________
't : .-.c vlk?J!.&---------L........;;sv. s t ar t ..................____________ ____es t . oowi?;.Enr;w_ 3/25
_______
AU'.tXS:
Determination of money value and resistance to abrasion complete.
Requested by J. Jackson to repeat resistance to abrasion test and evaluate under moderate abrasion. Work is scheduled for mid-March.
HIONE2:-
DUP050081891
;;f
IMGmVGRY mPOiHWWT
GXGsmvr r.u.v
CUSTO M Tv!
WORK REQUEST NO "
. n .c -68-2 First & Pinal
PC-6803-P
DATE
3/19/68
DISTRIBUTION
V;.
j.
ft.
Ayi
t .
Srengeman/li.B. Ic.aiefc
T ,B* S\Z>:''V<3
HP,
tolo {4}
Pigment's, C,B. File
Clark,
C.R.
P.D, Graham (2), PIgm., Wilmington
R.H. Yabel
"
VI,S. S fe ru v e/A.A.Briazo lara, Newark
H. Ar-noul
"
J, Jackson .
11
H.R. Linton
"
FajMRcsjs y e l l o w Y.-790-D in p o iy s t y r e n e XNP.it OLuCTION
Research submitted Kralox0 Primrose Ye 3/low Y-790-D lot SW-OO282 (50^ polystyrene .laked) to determine heat stability and resistance to abrasion in general-purpose polystyrene, and economics versus ca dm'lum. Krolox^ Yel3.ow Light Y-781-D was used as the con trol for heat stability and resistance' to abrasion tests.
CONCLUSIONS
..krolor Primrose Yellow Y-790-D is not considered a suit able Krolpr^ release due to ^considerably poorer heat stability and resistance to abrasion than Krolor Yellow Light Y-781-D. On a commodity basis, four times the Ida d ln.g ofacadm lum of comparable shade would have to be used'to'obtain equal depth of tint,, and equal hiding in masstone (Tables I & II).
Exhibits have been provided J. Jackson.
MM&,JMM3S..
'
Heat stability was compared under moderate and high sheer* didporslon, Dispersions were prepared in the Danbury under high Shear cohdltlpi'isv using a hand stirred charge oH color (13 gm. iCrolt pigment basis) and general-purpose polystyrene pellets (HOG gm.); two similar charges were dispersed.
The Banbury was operated as follows:
Run at second speed for one minute; stop, raise ram
and brush down loo%e -pigment to chamber; lower ram and operate for one minute at second speed; stop, reverse speed for 15 seconds; run
v. .ft v.ti umnTn / w
DUP050081892
HC-6B-P
2, 3/19/68
forward at second speed for additional minute; drop charge, cut and chop.
Dispersions were prepared in the Banbury under moderate shear as a 15 phr concentrate in general-purpose'polystyrene. Pigment (150 gm,~iCroloxd> pigment basis) and resin (1000 gnu) were
combined by hand stirring, and charged to the Banbury. Processing
was similar to nigh shear Banbury cycle^ The concentrate was let down to 1 phr in a 3 minute Banbury cycle.
Heat .stability was determined In the laboratory Van Dorn injection molder, using a continuous molding procedure (one chip per minute) so that chip numbers 16, 29, 42 and 56 represent
approximately ten minute, dwell times at 450, 500, 550 and 600 F., respectively'; chip 3 represents minimum hold time to reach color equilibrium at 400 F, (approx, three minutes).
Typical molding conditions were;
Plunger forward '
15 seconds
Mold closed
45 "
Booster
off
Bam pressure
500 psl
Ram speed
green
Spreader
40.rpm
Mold temperature
ambient
Mold, single'stair chip
Comparisons for tinting, strength and hiding were made in
geaeral-puroose polystyrene versus-a cadmium of similar hue. Pig ment vias added to fluxed resin on the two-roll mill, and dispersed under high shear. Comparison was made at 1 phr masstone for equal ftidlng and at .1/ 1,0 phr color/R-XOl titanium dioxide at equal depth of tint. Presflouts were prepared on the laboratory 50 ton press.
Pigments Evaluated Krolor"5 Primrose Yellow Y-790-D, SVf~00282
Other Pigments Psed
Krolox^ Yellow Light Y-781-D S.L-86728 Harshaw's Cadmium Primrose Yellow 1465, C-65129
Other. Hat la,, Used.
',
Dow's Styron 666, 'general-purpose..polystyrene pellets
HSSegBSHfiBB
NO-68-2
,
.
PC file 6803-P (L. Dlngess, D, Frank)
'
CHAr.SE; > 8253-4671-700
H.F.B.
DUP050081893
m
rH
p r
0oo
43' to
oRo
d 0 d
' ' V
rH 43- rH
0
.4
in
PO
f--1
0 ~oor
onn
'8 *i SO
o cn
d m*
d W
o * m
00u<KvPU>5-*'.i;
m
>CO *Hn
o oolA
roH 5
rrHrl So40O3 Ors
d 00
X)
T3." d
r VO
so*
T3 o
d in
m d
d >
VO
0
9
43 <fSl>j
in
s os CO
* CO
* s-
m.n
&f- ta
00
rH
fl>
<M -0rRp!)
50
H
r--R0! o0
H4003. 0OO!
S3
`r-l
R RfcO
rl Of 3o*.
m6u
4r3 0Sfch!O HRfMt*
0!
0
rl
so
; _j..<*
NHr
VO
*v-x
* 43-
.S*-
ra
MUR/v ;.
R CO
^ . *-
t0o . : 5
H w
P
:,-.A . H>
:c
'ft
ft
H
5
m
R p w
43
54 d o
n
CO
O
43
0ri
0.Ps0H11Si
9 OOs1S-' X
p *#: C}sMO1-
p1. ' SSS;"
i s
po1 OS1S,s
roa.
&1 0
R R 4>3
0 ra
rH 0}
*
> H
ra Q
CRD 1(10)
R -P
*
43 0
rH r-t
Rrl
bDP rH
0 !h
Cd
0
rl 3
0 a
El rH
43 SI O.
0
Ih
o
43 43
rH 0 P
Hp
ca r-^
R
rP R
H rH & rH O O
d Q.
43 <H
0 -d
43
a
0 n
43
43 53 rH
C 43
*
a 43
ft rH
>>
ra n Hr .43
fcO ct &2
' (3 g oo
403 d
pp
s rH 3! ra
a <H 043
il It
o 43
43 rH ra
43 H
VO o rH O 43
O rH
U <H ,
S2
Ou rH R o
< a
43 t( 0 0
0 43 P Or ra
H H
bO,40
O 43 3 43
-rl rH
>> U
in rH
rl
R
CQ > 0
. H
43 ra
0 "d h a 43 oc rH f-3
S43
ft 43
O 5h 43 S3
Oo
II II
oco cu
43
S3 H
bp
R
rl W
oR
R H
ra
RR
O
43
0 R
H 0 EStJ
ri
O ?L' <n > 4a
o
*svoo 4oMr>
i ii ii
53 SO
Oxt
H
s fcc
oe
<H O
nrl ih
43
rri 43 S>
oR
7 rH
43 H Hip
t'W
H Sir
# St .
H Kl 0
r0a rl
b~ w
r0a
xs
i
H d
R
0
4ra3
>> 4 3a
ra
u 43
0
p 1
S-, o
4s3>
rHH
C!
H fr
43 >*
43
43 6)
m >
rH
43 O'
0
{2}
0 & O
P O*3 p & .S3 m
4o4
0rH C-i
,C! O
o H <14
om
m
p
bo.
Co A
D
wR
1
40
R CO
S4O0
43
43 bHp &3
R
d o cp
ra H
rRa
rH
#!' 4>
rl
HR
/s r-7 H PJ ro
*>-** wr^s m so_
DUP050081894
TABLE I I
***.
' H':'
HAOI -
CM
OA
*8>
Economics - K rolox^., v s . Cadmium
m j3 X aa
i XrSl
0
S
-P
%
1 <H
OJ
oCM ,
*ri
IH
ft.
P AH
HAO
AO
o
AAA AAA fH T"l \l--1 \ 0" oo
**s. **=wt
IA
PS03 A>E6rCi
-H0*WH*' oT
JO3S oCf\
lJa'sl }H1
aoH.
A0KA
Xr)f
jAH
0 a> pr>a3
P4Ar>l <A
HO 0
0in** -oo9-
!
a . u0AOA3Oir
rCA-Tl) 0A0) fcO
*SH3,
P
0A. d *SO-)i oo
fseO
ri
*}
ArS*
H <P8 0o-
ra0cP*!j`
-P 0
'P 0
-V=irnO*?l SO Hr*l s* <a,
a
*0aH Aa
0rt 0
0 E
03 8
SO3 So3
CO Sril
EHQ,
Si
0Or OI -
0 (a o
Or o
0 X0f
a0rl
$ an
Ap0 o0
rr-l
Si 0
'
S2 1
A ao ;
fAO 0
o a?
,rv vrH>* CM co ,0-
DUP050081895
CC: W.P.Spengeman, Chestnut Run .
H.B.Clark,
""
S, J, Gorman, Wilmington
P.D.Graham,
"
R.H.Zabel,
"
M.Hunt/E.Gonick,
"
W.S.Struve/A.A.Brizzolara, Nwk.
R.A.Hageman/H. Arnoul,
"
H.F.Bartolo, Chestnut Run
JOHN A. LAMIET (2) Chestnut Run
Newark, New Jersey July 17, 1968
KY-790-D PRIMROSE "KROLOR" EVALUATION IN PLASTICS
We are forwarding to the attention of H. F. Bartolo, samples of specially prepared primrose yellow shade "Krolors" which are superior in thermal stability and abrasion resis
tance to anything else we have been able to make to date*
Since we have not been able to' evaluate Y-790-D types, extended with polystyrene in a manner that duplicates your findings on Y-790-D, 00282 (PC-6803-P), we are requesting
evaluation under high shear conditions in the Banbury before proceeding further.
The samples to be tested are as follows:
1. Y-7S0-D, SW-00282, control 2. Y-781-D, standard, control 3. 1877-39A Special toner 4. 1877-39B 50$ polystyrene lake of A 5. 1877-39C Special toner 6. 1877-39D 50$ polystyrene lake of B
r
As discussed with H. P. Bartolo, samples A and C and B and D can be combined, if necessary, to obtain adequate test quantities.
do
DUP050081896
0 DISTRICT MOR.
0SALESMAN
Q DIR. TECH. SERV. LAB (4)
VJ* F* - ooa*
t C f*
CtWTOMKR
mmr m
'PSMHWIW MIMNSW (LM.)
DISTRIBUTION
Bt e c h . MOR. `TJfTSjfc P*fl*<lrahws 0 EXPORT MOR.
COLOR* Plata* .tflltti PI mg r . t e c h . Wh it e s
_Kl
LAB.
DIR.
W53/AA2/00
RESEARCH
0SUPT. PROD. CONTROL
JAbill?f]OTHMR.B. flgta>.yilWs
raoriuc
CLAM W UK
' -
w.a no. K088-24
BtmtCT
DATS 7/19/68
ftALDMAM
COM0UETB WORK IV
COM^triTM
OBJECTi
COMPCTITIV* NAWK AHO COOK
" ' ($3X3 IHl REPLACES lv*5C*S4 1X&&) V/tS/Suf
8KU.INR RMCK
<
f BETAILROOSSCRIRTION OR WORK REQUIRED:
Svtluat* tha fallowing calico la pietctics as psr ltttsr JTHAL, 7/17/M*
' Ki~teo*:D s k *q 6C** control '
j
j
7*732*2, standard, control X87?S3A' Special fconor 1677*352 0$ polyatyrsn* lake of A v-. 2377*300 S'pocl&l tonar ' 2077*399 50JS pelystyrta* l&ks of B
I
. I j |
DUP050081897
f
:K.a.v
n. i v
I6MEHR! DPAS3Ti3EMT
cfttssnsur tsaes
FIRST & FINALpC ,c17?' - oo ye*
<~~DBFTPEH7I/U.
THIS REPORT IS FOR COSTOMER'S INTERNAL USE ONLY IT IS NOT TO OE COPIED WITHOUT THE PRIOR WRIT TEN CONSENT OF OU PONT
CUSTOMER
WORK REQUEST MO
PC-6875-P
DATE
KC-68-24
October 17, 1968
DISTRIBUTION
; : W.F. Spengaman/H.B. Clark, 0,R. 0.- Wormald* Pigm. 0.tR> V/.W. Riches, pigm. C.R, J.A. Lamiet, Pigm. G.R. T,t Reeve, Pigm, C.R, Pigments Chestnut Run File (2)
S.J. Gorman, Pigm. Wilm. P.D.. Graham, Pigm. Wilm. [&\n R.H.- Zabel, Pigra. Wilm.
-A. Brlzzolhra, Newark H, Arnoul, Pigm. Nejuark
T.L. Mitchell, P>gfn. C.R.
SUBlEcr ; SSPERIMEIfTAL PRIMROSE "KROLOR11 YELLOWS IN POLYSTYRENE
INTRODUCTION:
We evaluated experimental Krolor Yellows in polystyrene to deter mine thermal stability under high shear dispersion conditions. The following 'experimental pigments were evaluated in general purpose poly-
'-39-A 1877-39-B 1877-39-0
1877-39-D
Special toner (100$)
50$ Polystyrene lake of A Special toner (100$):
)$ Polystyrene lakeof G
Kp
fri.
Previously evaluated Primrose "Krolor^11 Yellow, KY-790-D, SvJ-00282 was included as a color control and "Krolor^" Yellow Light KY-781-D, SL-"~ was included as a heat stability control.
CONCLUSIONS:
.
The experimental'lake sample, 1877-39-D provides the best color and heat stability of the experimentals tested, but a toner which would combine
the more desirable primrose color of KY-790-D with the degree of heat stability shown by 1877-39-D wou1d offer much broader application and
acceptability in plastics.
Reg. U.S. Pat. Off. - Du Pont
SIGNED
T.L. MITCHELL/,3ah
DUP050081898
V-' 1-Keat stability rankings- for these products tested under high shear dispersion conditions arc:
Good (8) 1877 - 39 P (lake)
Fair (6) 1877 - 39 B (lake) K7-781-D
Poor (4) 3F/~790~D (lake) '
Bad (2) 1877 - 39 A (toner) 1877 ^ 39 C {toner)
"2-^`Sh.e experimental lakes are decidedly more intense in initial color |400*F) than the corresponding toners, but still lack the desired
intensity and greenness of KY-790-D, .SW-00282.
BXB!SffliimS!AL
i
Beat stability -under abrasive, conditions was tested by Banburying - and injection molding under the following conditions:
Banbury Dispersions s
Kand-stirred blends of color end Dow s Styron 666~JC26~7 general purpose polystyrene pellets (1100 pm. resin/1,0 phr dry toner) wer$ placed in the Banbury heated to -250*~60'*C and dispersed as follows:
dun at second speed for one minutej stop, raise ram and * brush down loose pigment into chamber 1 loner ram and operate for one
minute a second speed? stop reverse speed for 15 seconds; run forward at
second speed for additional minute? drop charge,, cut, combine charges and chop. *fwo such batches of each pigment were made for heat stability testing.
Heat Stability:
Using a continuous molding procedure (one chip per minute) in the laboratory Van Dorn injection molder, chip numbers 16, 29, 42 and 56 represent approximately 10 min, dwell times at 450, 560, 550
and 600eF, respectively, with chip #3 representing the minimum hold time needed to reach color equilibrium at 400*1'' (approx, three minutes).
.typical molding conditions were:
plunger forward.
.15 seconds
Mold closed
' 45 seconds
Booster -
OFF
Ram pressure
500 psi
. " speed
green
Spreader
40 rpm
Mold temperature
ambient
Mold, single stain chip
DUP050081899
REFERENCES:
''
W.R.. NC-68-3 & NC-68-9 {PC-6S04-P ) W,R. NC-62-24 (PC-6875-P L. Dittgess) TF-6010-1
CHARGE: 8253~i!651-500
. . ` TABLE 1 mSSTOHE THERMAL STABILITY
Sample
Loading* . phr) "
Color at 400F
Heat 450 ^
Stability 500w
-v--s--.W400rQ~F
Chip**
ICy-790-I>
2.0
Control
7d
5d
3d Id
Primrose Krolox Yellow
K5f-78l-D VvtA wUi^? JKZ JL J.UvJ L
1.0
_ _ _
8d 6.5d 4d 2.5a
1077-39-A (Toner)
1,0
Lk., red,
7d
dull., vs, opaque
4.5<J
2,5<1
0
1877-39-B (lake of A)
2*0 RedjS.dk..s. 8.5 dull,vs opaque
6d
4.5d
2d
1877-39~C (Toner)
1,0 V.Dlc,, dullj 7d 4d 2d 0 red, vs., opaque
1877-37-R f lake of C)
2o0 RedjS. opaque> 9.5 vs.dk.j-vs, dull
^Equal tone** loading. *See Experimental Dei;ails
8
6.5d
4d
DUP050081900
W.S. Struve/A.A.Bri*uolara, Mwk.
D.E. Yonker, C.R. (2) H.F. Bartolo, C.R. (6) W.VJ. Riches, C.R.
B.J. Godfrey, Pigm. ; lev/ark P.D. Graham, Pigra. Wl!nt.(2) Pigments, Chestnut Hun Pile (3) C.G. Quinn, C.R. (3)
E..F. IClenke, Plgm. Newark
----J . J . Jwau cvJkXOsowUn, P1 XigKrlaU.f Ni iVenwark H.II. Zabel, Pigm. Wilm.
SERIES P-6880S
TNTO/lirRE'P9R^'~ (Ref. w r . m=&r=&7$r^B} n c -68-2)
Chestnut Run October 2, 1968
KROLORP AMD CADMIUM PIGMENTS IN PLASTICS
OBJECT;
Compare durability of Krolor^ and cadmium pigments in resin systems.
ffesstone and tint swatches .(1" X 5"). of cadmium and Kroloi^5 pigments, prepared at equal opacity and 'depth of color in polyethylene and polystyrene, are being exposed in Delaware for examination at o mo. intervals.
REFERENCES: NR.NC-67-33,34,38; NC-68-2 PC-6799-P, 67100-P, 67105-P, 6803-P
CHARGE: 6606-200
'
Krolor Orange R K0-786-D lot 52197 Krolor Yellow Medium ICY-787-D lot 52569 ^--wj^Crolor Primrose Yellow KY-790-D SW00232
liarshaw's ^Cadmium Yellow 1465 C-65129 Harshav?1 s"Sa dmiura Dark Orange 797-H C--54471
Imperial's Deep Cadmium Yellow X-2826 0-65401 Harahaw's CP Cadmium Red Light 1410 C-65107
EXPOSURE CONDITIONS:
45S Delaware,' 1 set-readings at 6 mo. intervals
R. F. BARTOLO PIGMENTS TECHNICAL SERVICE LABORATORY
Jah
DUP050081901
ift i-S I in P=i rH
tx, oIn
P-i* 01
oQrHJ
O C-r fft VO
vo 5
0.1/1.0
1.0 1.0 1.0
K ra lo r KO-789-D Lot-52097 Cad. 1410/Cad. 797-B (1 /1 ) K rolor KO-789-D L o t 52097 K ro lo i*3 KO-789-D L o t52134
.rH
OrH 0
0
'i -
(S3:
\
ft
fftt
O
0
r-I in 1--1
v. -=f
O
O * r-5 .
Q
rH N>
ft-*
\ r--1 in \
Q
in r-i
\
OJA rH
r~!
t H.
H
r*3 -=i-
rH. ' 0
r-i *
r~j
r~l
r-I
r-I
0
o{
O
0 0
O
s
\ 1--i
hi H M P
<C S3 &* a>
p Si
- (L
10 vo
CM CM
CO CO
CM1
JH
kCrHMa1
w
.1
g0
r-i
f1i 0t~0.
O r-i r-i
P !
CO
in VO
ft-
rH
P1 O0\
vino
H
P
1
Ocn
p I
0VO0
o to si
r-
1
H trf
ft
ft
0
A r-H
fOt
P fed
i
&
>4
ft
mft
A
0
r-i
Oft
IS t-1
OH
rH W
l-l 0
Pi
Kf>'t
r0-!
CM
Pft
ftj
t1-
ft3
O >1 0
H i4 S4
rH 9
<U J>*
ft
$ft
k.A
s
*
1--Oi
O H
CM
f0t
0ft
CM
w
O-
CO
rH
n r-1
\ -.0 p~I 0
p
O
P
1
VO CO
t--1
rH ft-
Wi
rH 0["1
S>
P
p
0t\
co
r-
1
0
n.
P fcO c ft
V. /T
ft P ft ft
O OO
pH
f0t
O . cM P
rH
HO
P
ft Jo
n ,
^.e
^'
m rH
;- -
ft ft
'Tr>v-. *jg* ' ' >> rH w (ft
n
0
fc'-
B
P ft
CO .JO
CO
VO
RX1t :
"
-.SK W
rH CM tn Hi- n vo c- co o n 0 rH
. r4.. r-i
r-I rHt
M%
DUP050081902
W.f. Spcngeman/R, J. Fahl, CR. G.. Worms'I d,,. C, Ro
A,, Lc.nie *">> C R * AF,, i@wf.Sf CoRo DoSo Yonker, e,R,, (2) HuFo Be"tolo, CoRo (6) W,W Riches, C R R.H, Zabel, Pigm.., Wi 1m,
W.S, Struve, Pigm,, Newark
(3.J Godfrey, Pigm., Newark P.Do/^ahem, Pigm*,, Wi 1m. (2) IPtetmentS'ffesRun File (l)
^CoGo Qbfnn,Vc<lf, (3-)--^
E.Fo Klenke, Pigm,, Newark JoJ. Jackson, Pigm., Newark
Chestnut Run June 2.3, J9&9
SERIES J3-4Sg06) INTERIM; REPORT (Ref, WR. MC>T7-33* 34, 38; MC -63-2)
KRQLGR AND CADMIUM PIGMENTS IN PLASTICS
6 Months* Report, Delaware 45 South
INTRO DUCT aJM :
'V
K 'olor pigments are compared with cadmium pigments of simitar hue in masstone anf tint in pclyethyl&ne and polystyrene; 'exhibits ar scheduled for evaluation et 6 month intervals.
coitus JONS
Based or the limited exposure, no significant differertces are noted between Krolor and cadmium pigments of similar hue In either masstone or tint , vmutation, Examination of the exhibits is scheduled to continue for a 36 month exposure period. Color failure is generally more severe in yellow hues than in the oranges,. Failure in tint formulations was gen* era ly more severe than in masstone formulations,
EXPERIMENTAL DETAILS;
Sources of detailed information on exposure and preparation of ex* hibits ere listed in the initial report on exposure series P*68806,,
CHARGE; 6606-200
* H, F, Bartolo PIGMENTS TECHNICAL SERVICE LABORATORY
1#'3 smal Attachment
1
Registered US, Patent Office' - Du Pont
DUP050081903
SERIES P-68806 Interim Report
Exhitilt ; -i
2 3 4 5 6 7 .8 9 1 ti 12 13 14 15 16 17 18
TABLE 1 * DURABILITY IW PE & PS^
?foment Harshaw X-2826 KY-787-0 Harshaw X-2826 KY-787*0 Hershew 1465"01 KY-790-D KO-786-O KV-790 -0 KO-786-0
Loading, phr (Color/TiOu) 1.0 U5 ... 0,10/1,0 0,14/1,0 1,0 4,0 0.15 0.4/1.0 0,15/1.0
6 Mos,, 'Bel.. 45 S. S* d vs less int. 9, d vs less int. 7, d si.less int. 8, d less Int, 8, d red, less int 5. d red.less int. 6, d red Al - d red 6, I
Hsrshaw 797**H Hafshevr 757-H KY-786-0
0,10/1,0 1,0 1.5
7, 1 s d vs less int. 9, d vs less int.
Hsrshaw l4lO/797"H
0.05/0.05/1.0
7, 1
K0-789-D, lot 52134 KO-789"0 lot 52097
- 0.10/1,0 0,10/1,0
7, 1 si less int. 3> 1 si less int.
Hershaw 1410/797~H (1/1) KO-769-0, lot 52097 KG`-789-0, lot 52134
1,0 1.0 J ,0
3, d vs less int.
8, 1 s less int.. $ yellow
9, d vs less int.
U) Degree of Changes 10 nones 8 - slight? 6 ~ considerable? 4 = bad? 2 = v bad? 0 * complete failure. d s? dark? 1 light
HFBsmal 6/23/69
DUP050081904
E. I. DU PONT DE NEMOURS AND COMPANY Pigments Department cc:
S.J.Gorman, Pigts.,Wiim.
L.F.Andrews, "
"
P.D.Graham,
"
M
H, ArnouX, (2) Newark
M*Hunt/E .GonicK, " Wilm.
w.s.Struve,
Newark
E.F.Klenlce,
w
J. Jackson,
w
R. H. ZABEL PIGMENTS
WILMINGTON
Newark, New Jersey December 30, 1969
KY-790-D - HISTORY - CHESTNUT RUN EVALUATIONS
EXPERIMENTAL SAMPLES
At the October 3, 1969 meetingof Production-S ales-Research,
a request was made of the writer to summarize the history of the above subject.
Ref. 1 JJ - J.A.Lamiet Y-790-D Primrose "Krolor" 1-10-68
This request for the evaluation of KY-790-D, 00282 (a 50% extension based on polystyrene) was reported out in Ref. 2.
Ref. 2 Work Request NC-68-2
3-19-68
The conclusion reached in that report were:
a) "not considered a suitable "Krolor" release due to considerably poorer heat stability and resistance
to abrasion than "Krolor" light Y-781-D (KY-781-D - SL 86728);
b) "on a commodity basis four times the loading of a
primrose cadmium shade would be required equal depth of tint and equal hiding, in masstone" (Harshaw1 s Cadmium Primrose Yellow 1465 used.
Priced $3.95 as of date of report).
The above conclusions were based on Banbury dispersions. Details of readings are given on the attached Table I.
Additional laboratory studies were conducted in an attempt to develop a more suitable primrose yellow base
for the manufacture of a*"Krolor" pigment.
DUP050081905
KY-790-D
-2- December 30, 1969
Ref. 3
JJ - J.A.Lamiet KY-790-D Primrose Yellow 7-17-68 Evaluation in Plastics
This requested the evaluation of several laboratory samples (NB 1877-39A B CP) versus KY-790-D, 00282 and
KY-781-D. These samples included two experimental toners and the corresponding 50% polystyrene extensions* The products were strictly experimental and would require . the development of a 12 Bldg, process to manufacture the basic yellow.
Ref. 4
Work Request 68-24 summarizes the findings on these samples. The conclusions reached were:
a. "The experimental sample 1877-39D (50% polystyrene lake) provides the best color and heat stability of the experimental tested, but a toner which would
combine the more desirable primrose shade of KY790-D (00282) with the degree of heat stability shown by 1877-39D would offer much broader applicat
ion and acceptability in plastics."
For details see Table XX.
These conclusions again lead to the conclusion that
a) lakes are objectionable although they gave adequate thermal stability;
b) product excessively red in hue;
product would require 12 Bldg study.
Ref. 5
KY-790-D, 00282 was included in a-vrnyl dispersion study P-68806. Six month data indicates a large inferiority versus "Krolor" such as KZ-787-D (Cvs. 8) at six months
On the basis of the above it would appear that the maxi mum selling price that.'Could be put on this product at the time was in the order of $1.00/lb. Various discus
sions with Production, personnel lead to the conclusion that this process was not attractive, and no further work to develop this type material was undertaken.
In the light of current price and supply problems with cadmium yellows, these conclusions might be altered.
mm Attach.
JULIUS JACKSON RESEARCH DIVISION
DUP050081906
o p
ovo
eto
0O
oitnn
5>
i0
X13 r-H
133*! 't
3U4 r-t
Jg
in
c*>
13
1a3:
1X3 0
X V
vb pi m c m in
H4* 3
in
r; K0
44 o
rt
rt
oin
m <
CO
13 Oi
13
S
vo VO in VO
CO
& *3
13
0?
13
0?
r>
in
CO
ES a< H s
H O VI 43 rt O O
r-l 0O 6O o
iH 0 H
4rJt
0 o
<u
irrntt
p
4-) r-l
w
C H
rot
rt -l
.
rt
rPt
o
<0
r<ut
co
rt
<<00 o o rrtt
c> ohi
rt rrtt
0 rt irl 3S to CO rt
S' to w rt
PCl rt m 1 eg So H
rrtt
rrtt
rt
(0
rt
rt
Xrt rt rt rP
.rt X CO
co w co
X rt
rC X- S>
tn tn
H M
Q
to to w M
HI CM 03 CM
y p p P 4J P
S3 rt rt? rt ' o '
ui CO co w to
<*>
PS
CM o l r* 1
orrt V0 o i--!
o
sid* 00 00 OV CO 01 <n
12 r-* rrt 1 p j ) 1 l
JW CO
p* >|
:abi
500
&
rl
6O
fci s
o ost* . in mm > 1? Hrt
CO
arPst Q*ms*
oto OO3* X
fti
HrOot
#m
H CNJ
ONO'sf
in in in
CO
m ^ rv v>
*a m in
m vo <4< io d< co
uXrn m
*
r- co r- co n ov
u
%
rt
. rt
rt
rt O'
t-o
Prgt'Oto
rtot rrHt
0
Xrt oto >rt CO M
1r3t m H 13
0 ,-s > 0 rt CO
0 13 13 M >
H rt H
0 *Vi H tO * *
4VJi PSQTrt Tr3t * ir-4l 1jM?
C >C X 0
OO 0-H rt 1r3t 13 13 M>
X Vi w .
p n
jx -
O rt j u 13 *0
d 13 >,04 p<0i t> trot
S* CM
1 CO so
a
w
p H
Em M
tn
a
rl 13-
S) K
Q P to
rt H to fD C0
oo 1*
CM i-l
+** .
CO CM
CM l> CO
PCM 1
O VO'WCO PQ
1l O trt
cr> ax o t> JJ
as
oo *
O CM O CM #.>s
r4 rtj rH Q IW
IP o 0
+* P M KW vi to vi ,, rt rt ^
o0 o ao om
EH in E-I
X ra o Q
cv ov cn cn ro m m
III! l> n- :f> tsc C' r- r> is
CO CO CO op rM i--{ rH rH
DUP050081907
o
U
Cu *
two J<asS
GO i^Iz *5
3 Sr* *
+-4
.g CO
-of
<
5
s
O
>5(Z>?*-.*f-^N2. >""g!>'
*
8' W
&o <U
z
I i
DUP050081908