Document qmkpwa0RqB3XkZpn1EegNmb25

_______________________ bulletin no iC/FF-38 TRANSFORMER Inspection & Maintenance Guide i Monsanto i i i t * i LEXOLDMON003184 SECTION A TRANSFORMER ASKARELS..........................................1 I. Introduction...........................................................' II. Hiftory of Trade Name Type*..............................1 Table I - The Composition of Transformer Askarels .......................................... 2 III. Interchangeability ................................................ 2 IV. Table II - Official Transformer Adcarel Shipping Specifications........................................3 V. Ordering Instructions ...........................................2 VI. Stability.................................................................. 2 VII. Precautions Whan Handling Drums, Tank Cars and Whan Opening Transformers........................ 4 A. Keep Dry During Handling ...........................4 Table III - Handling and Pumping Temperatures.................................. 4 B. Use Ordinary Personal Precautions ..............4 C. Precautions on Opening an Askarel Transformer........................................5 VIII. Avoid Environmental Pollution...........................5 1. Labeling Askarel Transformers..................... 6 2. Disposal of Liquid and Solid Wastes ........... 6 3. Conditioning of New or Recycled Askarel .6 4. Teardown of Transformers for Repair or Scrap ........................................7 5. Transformer Disposal..................................... 7 IX. Expected Service Life...........................................7 X. General Characterretiee4Transformer Adtaral Fluid............................ 7 XI. Sampling Transformer Adcarel Fluid ................ B XII. Evaluation of Adtaral Received in Now Equipment............................................... 8 XIII. Dielectric Breakdown Voltage - Moisture Ralstiondiip.......................................... 9 Table IV - Relation of Dielectric Breakdown Voltage to Amount of Dissolved Water in Askarel and Mineral Oil........................................9 Table V - Approximate Solubility of Water in Transformer Askarel and Mineral Oil .... 10 XIV. Turbidity ............................................................. 10 XV. Chock Points for Maintaining . Adtaral Insulation ............................................... 10 * A. General Considerations.................................. 10 B. Modern Sealing Procedures......................... 11 C. The Older Sealing Arrangements'.................12 XVI. Periodic Fluid Inspection and What Chedcpoints Mean ................................... 12 A. Visual Inspection....................................... 13 B. Dielectric Breakdown Voltage ................... 13 XVII. Inspection Checklist..............................................13 XVIII. Contamination in Transformers.........................14 Table VI -- Effect of Common Insulation Materials on Power Factor and Dielectric Strength..............................................14 Table VII - E'fect of Common Insulation Materials on Volume Resistivity of Askarel............................................................. 14 XIX. ASTM Method for Investigating the Compatibility of Transformer Insulation and Construction Materials in Askarels............15 XX. Refining Askarel for Re-Use..............................15 A. Filtering Through Dry Blotter Paper to Remove Moisture and Extraneous Particles............................ 15 Table VIII - Water Removal by Filtering Askarel Through a Paper Press ......................... 16 B. Disposal of Solid Wastes .............................. 16 C. Solid Insulation Requiring Drying.............. 16 D. Earth Treatment for Maximum Improvement of Power Factor and Volume Resistivity ......................................16 Table IX - Effect of Power Factor and Volume Resistivity ......................... 17 XXI. Cleaning Arced Transformers............................17 XXII. Sampling Askarel................................................ 17 SECTION B ASKAREL FILLED SWITCHES AND TERMINAL CHAMBERS .....................................19 I. Introduction.........................................................19 II. Sources of Contamination .................................19 III. Sealing Switches and Terminal Chambers...20 IV. Askarel Used Under Mild Arcing Conditions . 20 V. Maintenance for Adcarel Filled Switches . . 20 VI. Askaral Under Excessive Temperature or Fault Conditions ...........................................21 SECTION C ANALYTICAL SERVICES ON TRANSFORMER ASKAREL AVAILABLE FROM MONSANTO................................ 22 Types of Analyses Available: ........................................... 22 1) Routine Maintenance Check......................................22 2) Complete Analysis..................................................... 22 3) Analysis After Earth Refinement ......................22 Appendix A -- Askarel Stability and Composition of Arc Formed Gas...................................23 Appendix B - Solubility of Gas in Transformer Askarels ..................................................... 23 Appendix C -- Effect of Temperature on Dielectric Breakdown Voltage of Askarel ................... 23 Appendix D - Comparison of the Approximate Viscosity in Saybolt Universal Seconds of Transformer Askarels and Mineral Oil........................... 24 Appendix E -- The Density of Inerteen 54201 KA 7336-9 and Transformer Pyranol A13B3B-3...........................................................24 Appendix F -- Thermal Conductivity Values of Transformer Pyrarol A13B3B -3................................ 24 Appendix G - Heat Capacity........................................... 24 Appendix H -- Coefficient of Expansion.........................24 Appendix I - Fire Resistance...........................................24 Appendix J -- Seals, Properties and Procurement ............................................................. 25 Appendix K - Caution Label........................................... 25 GflRN 000901 LEXOLDMON003185 fetffkmA Transformer Askarel I. Introduction . The term "askarel" es defined by IEEE, ASTM and the National Electrical Code generally describes a broad dan of non-flammable tynthetie chlorinated hydrocarbon insulating liquids widely used in transformers, reactors and eeeetsory equipment operated at power frequencies. Askareit of various compositional types are in use. (For the general properties and types sea -ASTM 0-2283.) Under arcing conditions die gases produced, while consisting of predominantly non-combustible hydrogen chloride, can contain varying amounts of combustible gases depending upon die askarel type. This manual describes the operating characteristics of transformer askarel liquid insulation and how it differs from mineral oil. Appropriate handling and disposal procedures for both scrap askarel liquid and impragnatad solid materials are given in accordance with the guidelines recommended by the American National Standards Institute. The information is based on facts gathered by Monsanto over 40 years as a producer of askarel, plus knowledge gained from the experience of transformer manufacturers and users. This guide outlines the very simple maintenance required for askarel fluid in "modern" transformers and offers suggestions for sealing and maintaining askarel in old units. By following this guide, we believe users will obtain maximum service from askarel insulation with a reasonable minimum of maintenance. If questions arise relating to the designing and building of transformers, these should be referred to regular transformer suppliers. Monsanto gratefully acknowledges the assistance, guidance and the contributions of certain data by the following: Edward L. Raab - General Electric Dr. T. K. Sloat -- Westinghouse Electric II. History of Trad* Name Typos "Askarel" is the generic name for the non-combustible liquid insulation and coolant first used by General Electric Company in 1932 for their Pyranol* brand name fire-resistant transformers. Westinghouse Electric Corporatio^mes tfair brand name, Inerteen.** Whatever the trademarked brand, the askarel contains chlorinated biphenyl -- one of the best liquid insulations developed by science. This inert material it* chemically stable, fire-resistant, heat stable, non-corrosive, endj has high dielectric strength under the operating conditions encountered in transformers. In addition to manufacturing Arodor* (chlorinated biphenyl). Monsanto alto mixes this dielectric fluid with chlorobenzenes to produce the presently used Inerteen and Pyranol blends described m Table I. 'Trademark ef OeHerat Clestrtc Company "Trademark of Weetlwpwua Eleetrc Corporation keentorod trademark of Sternerto Company UBRN 000902 LEXOLDMON003186 TMI Tlw Composition of Trendonnsr Adcard* .. . Method ASTM 02X3 LtPtP TypeE Tv55* . Trade Names Inertaen 7000 Inertaen 10042 Pyranol A13B3B3 Ingredients (% by wl.1 * Arodor* 1254. pentechlorobiphenyl 70 w* - 00 Arodor* 1242, trichlorobiphenyl trichloroberuene tri-tetredriorobenzena -- 100 30 . -- ---- -- 40 -- phenoxypropene oxide nmir 0.18 to 0.22 diepoxids scavenger Mthod ASTM 0-23X3 pendtip a 18 to 0.22 0.115 to 0.128 ASTM Method 0-2283. tided "VMoriniad Aromttie Hydroemtom (Adan/sJ For Tnmformtrt", olio lint the composition of ail transformer askareis used at various times since 1932. Monsanto manufactures similar transformer aOtarel fluids in England where the trede name Pyroctef is used. j i '. : ! | ; I i j - I. - III. IntarchangnbiKty In general all transformer askarets are interchangeable. However, h is auggestad that the transformer manufacturer be consuited prior to mixing in significant proportions or total substitution. IV. Official Transformer Atkaral Shipping Spocifieetioni The official dripping specifications far the three modem transformer edterel fluids are shown in Table It. . V. Ordering Instructions Monsanto's current policy is to all adtaref transformer fluids only to transformer manufactum Others intirested in thew fluids dtould contact the manufacturers of eskarei transformers and not Monsanto. The transformer name plan indicates the trensformsr maker and usually gives suffieiem date to identify the specific adtard fluid wad. . . _ . VI. Stability ': Asfcarel liquid insulation h highly pure, fire resistant liquid made under dose chemical control to meet the exacting specifications as diown in Table ll. lt dosems veri bycampoaklBp 9ha tire commerdei tengeaf. . tninerd oils. . _ . . . ' .. ' '' . Aakarel insulation must never be werad with mineral dt. Deer two . /. percent of miianf oB by volume in adcard begins to lower id fits' Askerd does not dewiuiaie whwi evpoeed to air, boat hot mold; k tee not bredt down oeor long uto to form conducting ar Aakard wiD remain .___ . broken down by swam ............... '* *i ^T*iX^*****:"*"' ' v ^v"11 i bmiiiiiir'T-r- Mr. ff neior te '|t ve^wd irr/rt`ri,4u8jl. ' - '-J-'' " . .. lexdi ni\/inMnrmR7 LEXOLDMON003188 CD 3D O O O <o o <b?) . Table II Official Transformer Askarel Shipping Specifications SptWcUlm fropartfcs Color.'APHA vhfnndition ` sEar com*nt. ppm (ASTM D163360) *lcidily, mg |COH/g (ASTM 0974 55) Dielectric Sirangih, 25%, 0.1 in. gap (ASTM 087749) OMectric Constant, 100%, 60 Hi (ASTM0924 49) ? *. Voluma Resitlivity, 100C. . 500 volts DC 0.1 inch gap, 109 ohm-cm ' (ASTM 01169) Inorganic chlorides, ppm (ASTM 01821 and G.E. Method E4C41B) Retractive index. 25% (ASTM D1807) Viscosity at 37.8% (ASTM 088 56) Sayfaoll Universal Seconds Pour Point % (ASTM 0 97 57) Specific gravity 25/15 5% (ASTM D1810) Burn point (ASTM D92I Distillation range (ASTM 020-56) corrected lor stem and barometric pressure Generel Electric Co. Transtormer Pyronol A138381 ASTM 02283 TypeO* 150 max. Clear 30 max. 0.014 max. 35 KV, min. 4.2to4.6 100 0.10 max. 1.6110 to 1.6120 44 to 48 -38 or lower 1.495 to 1.510 None to boiling 1st drop 200*C min. 40% max. below 270*C 90% 379 to 394 Transformer Inanasn 7030 ASTM P22t3 Type O 150 max. Clear 30 max. 0.014 max. 36 KV. min. 4.2 to 4.5 100 0.10 max. 1.6153 to 1.6173 56 to 61 -30 or lower 1.518to1.S28 None to boiling 1st drop 200*0 min. 35% below 270% 90% 379 to 384 Inerteen 10042 ASTM P2283 Ty^e E 60 max. ' Clear * ', 36 me^H-i. . 0.01 IM8. 36 KV. 4.7 100 0.05 max. . 1.6240 to 1.6260 82 to 92 -17 or lower 1.381 to 1.392 None to boiling 10% 325% min. 90% 360 max. ~V V, Fixed chlorine 56.4 * 0.5% 56.6% min. 4310.5% Corrosion test After heating with aluminum for 6 hrs. at 200 to 220%, the aluminum must not be corroded ' on either visual or weight inspection and the askarel should meet the following specifications: -| Color. APHA 200 max. 200 max. 200 max. Acidity, mg KOH/g 0.014 max. 0.014 max. 0.01 max. . Inorganic chlorides ppm 0.15 max. 2J0max. 0.15 max. ' Condition Clear Clear Clear Scavenger content Typicil Properties < Coefficient ol Thermal Expansion 0.115 to 0.135% Diepoxide 0.0007 0.18 to 0.22% phenoxypropene oxide 0.0007 0.18 to 0.22% phenoxypropene oxidy 0.00068 1 (ASTM 019031. cm2/cm2/C Arc formed gases Askarels ol various compostIiuiidl types we used. Under ocmf conditions lh gases produced, wluli constating \, `. predominantly ol non combustible hydrogen chloride, coo include eaaymg enounu of combustible inn depending*. *' upon the askarel type. Insulation systems mcoiporating these askarth and cellulotic or other organic meterial\mfy^, ' * When arced, produce gaseous mixtures which ere moderately flammable. As a precaution, such gases should 1 Method ASTM D2283 pending lot Type G. removed liom the askarel by bubbling dry mtrogon through the adtarel end Hushing the gat spec# with dry 0iU9fg|\ par bclorc any work is performed on the apparatus. 1 . i'.\ / , "Wsitmehouu ums tlMM privets number Inerieen M20IKA lor Incriccn 70 30 end Ihex puwlc number Ineneen M20ICM lot Insriacn 10042. u1. .' in a tiny mount (approximately 125 ppm) Swotvaa - tha raft float* on tap. Aifcaral is vary insoluble in watar, only about 200 parts par billion of adcaral ditaolva in watar, at normal tsmparaturas. VII. Precautions When Handling Drum, Tank Can, and Whan Opening Transformers Tha Anwriean Imtitutt of Electrical and Elaetronie Enginaan Guida No. 76. Daotmbar, 1958 has bacn revised to givs more datailad iretnictioni and guidanca "For Acapmrca and Utmunonot of Transformer Atktiol in Equipmont'. This guida it published by the Imtituta of Eleetricd & Electronics Enginaort, Inc., 345 East 47dt Street. New York, New York 10017. Tha following are significant preeautiont: * A. Kaap Dry During Handling: ' In handling, storing, sampling and impacting askarel -- and in operating adcaral transformers -- taka every precaution to guard tha askarel insulation from exposure to high humidity and moisture contamination. Keep 5 or 55 gallon drums of askarel dry; lay stored drums on their sides with tha bung at the highest point from floor to keep water off the drum head (which can be sucked into the askarel by the drum "breathing"). This precaution is not necessary when drums are stored indoors, which is the preferred place for storage. To avoid leakage the drums used for askarel are of heavy construction. Sixteen gauge metal is used, with special rim seal and bung construction. The drums should be drained as completely as possible and then flushed twice with kerosene type solvent to remove all of the askarel. Accumulated liquids and washings dtouid be collected and should be incinerated at hi0t temperatures, e.g,, about 2000f, to destroy the polydiiorinetsd biphenyls (PC8s). See Section A, VIII. Tank ears used to transport atkarelt are in exclusive service and not used interchangeably for other products. All care must be unloaded through the top (dome fitting) either by pumping or with controlled pressure using dry air or dry nitrogen. If nitrogen hat been used for unloading it is necessary to advise the shipper so that when the car returns the nitrogen can be replaced with dry air before any one may enter the car. If the car is to be unloaded by ptanping it will be necessary touaa dryer on the sir intake line to remove moisture. All tank cart are fitted with steam coils, whMi are available tar unloading under extreme low temperature conditions. Convenient handling and pumping tarnpereturn and the related approximate viscosity ranges are given in Table III. 5. Um Ordinary Personal Precautions: ' ' Transformer askarel has been made, handled, and used tar over 40 yean. It can be handled safely with recommended precautions. If accidentally spilled on hands, no serious skin irritation wiMoocur. However, liquid adcaral hat a meant anion (similar to paint Product Ttabto 111 Handling and Pumping Ta Unloading. Handling and . Pumping Temperature *C Pyrenol A13B38-3 Insrteen 70-30 . Inerteen 100-42 . . 30-55 - 36-76 - - Approximate Viscosity $US 100-40 WO-40 100 40 thinnarl on tht fas and oils of the skin and prolonged contact may laad to drying and chipping of the sktn. In CMC of contact, weds tht tkin with soap and water: remove and dry dean taturatad clothing. Clean up spills with rags, sawdust and absorbent day. Eye contact may result in painful irritation but no permar-nt damage to tissues. If eskerel gets in the eyes, flush with large amounts of water. As with all eyt first ad, refer to e physician. To relieve irritetion, physicians have used an opthaimie anesthetic solution as well as opthaimie cortisone acetate solution, or castor oil. Infrequent exposure to eskerel vapors will not cause iH effects. However, prolonged exposure to high vapor concentrations should be avoided. If hot eskerel must be handled in a closed or confined area, orovide the area with mechanical exhaust ventilation - or wear an organic cartridge respirator approved by the U.S. Bureau of Mines. C. Precautions On Opening an Askard Transformer: Askarets of various compositional types are used. Under arcing conditions the gates produced, while consisting of predominantly non-combustible hydrogen chloride, can yield varying amounts sf combustible gases depending upon the eskerel type. Insulation systems incorporating these eskarelt and cellulotic or other organic materials may, when arced, produce gaseous mixtures which are moderately flammable. As a precaution, such gases mould be removed from the askarel by bubbling dry nitrogen through the askarel and flushing the gas space with dry nitrogen before any work is performed on the apparatus. VIII. Avoid Environmental Pollution Transformer eskerels contain polychlorinated biphenyls (PCBsl which have been used' in the United States and elsewhere over the pest 40 yean for many industrid and consumer applications. During the pest eeveril years evidence haa accumulated to indicate that PCBs are widely dispersed throughout the environment and that they can have edverse ecological and toxicological effects, The United States Government's Interdepartmental Task Force on PCBs, Com-72-10419, in their March 20. 1972 report titled. "Polychlorinated Biphenyh and Ihe Environment", recommended restricting PCBs to use in capacitors and transformers. This report is distributed by the National Technical Information Service, US. Department of Commerce. Springfield, Virginia 22151. A document titled. *1auidatirm for Handling and Oitposel of Capacitor and Transformer Grada Atkans/t, Containing Polychlorinated Biphenyls"', has been prepared and is available from the American National Standards Institute, Committee C107, 1S5 East 44th Street, New York. New York 10017. - The scope, objectives and the composition of this committee are: ANSI Committee C107 Sfiopt: Procedure ard prides for safe toe. maintenance and disposal of askarel and askare!-soaked materials uead in electrical equipment. Objectives - ' . 1. Scarce of teehnied information and advice for Federal, Suae, local authorities md all others concerned. 2. Encourage development of aurtabte disposal facilities end heap 41 concerned informed. - 3. Sene as She advisory group for United States participation in international organiaationr. CEE, IEC, CIGRE. GBRN 000906 LEXOLDMON003190 Orgaoiutioot active in or represented by tbit ANSI commiRec include: National Electrical Manufacturers Association, Electronic Industries Association, Institute of Electrical and Electronic Engineers. American Society for Testing end Materials; Electric Light and Power Association; Certified Ballast Manufacturers Association; Environmental Protection Agency; Office of Environmental Affairs; General Services Administration; National Bureau of Standards; Department of the Army; Rural Electrification Administration; Division of Environmental Research, TVA; American Public Power Association, Water Pollution Control Federation; Food and Drug Administration; National Fire Protection Association; Underwriters Laboratories; and several sections of the US. Department of Interior. The following are pertinent excerpts taken from the ANSI Guidelines for askarel transformers: t. LABELING ASKAREL TRANSFORMERS "All new askarel transformers should be labeled: ^eution. The Insulating Liquid In This Transformer Contains Polychlorinated Biphenyls (PCBs). Care Should Be Taken To Prevent Entry Into The Environment. In Case Of Malfunction Or Leaks, Consult The Instruction Manual Or The Manu facturer. . The transformer manufacturer should make similar warning labels available for use on previously installed transformers." 2. DISPOSAL OF LIQUID AND SOLID WASTES "Disposal of askarel fluid and askarel-soaked materials must be accomplished by means in which there is no significant release of askarel to the environment. At present, disposal is accomplished by carefully controlled high temperature incineration of liquids and soaked software: and by controlled dry land-fill burial of apparatus and other hardware from which askarel has been previously drained and washed. "Present knowledge indicates that proper incineration should involve a suitable balance between dwell time and temperature in the incinerator plus oxygen availability and finally suitable scrubbers to remove HC1 formed; e.g,, 111 two-second dwell time at approximately 2000V and 3% excess oxygen in stack gat; 12) 1-1'A second dwell time at 2700V and 2% excess oxygen in ataefc gas." The ANSI Guide lists the locations of facilities that conform with the above requirements. Monsanto has such an incinerator at the W. G. Krummrieh Plant, Department A-246. Seuget, Illinois 82201. where arrangements can be made for scrap askarel liquid disposal for a modest fee, currently 3 cents per pound. For disposal of solid scrap a controlled dry land-fill can be used where permitted by Federal. State and local regulations. 3. CONDITIONING OF NEW OR RECYCLED ASKAREL Conditioning of new askarel or recycled askarel requires Fuller's earth treatment. The spent Fuller's earth in cartridges or begs whan replaced should be allowed to thoroughly drain * over drip pant to remove at much liquid askarel as possible. The cartridge units-of steel math construction should be , - pieced in the- "Saeet Contaminated with Askarel" container for disposition. Cloth begs filled with Fuller's earth should be pieced in the *3crap Burnable Askarel Waste" container for dispositions A GBRN 000907 LEXOLDMON003191 4, TEARDOWN Of TRANSFORMERS FOR REPAIR OR SCRAP a. Oram a(l atearel from th unit either into holding tank for rttia or into the drum labeled 'Scrap Askarel" for deposition, than allow wffietent time for all the atkarel , to drain from the core and coils. b. Ramose the core and coil assembly from the transformer and place it on the floor. Sufficient absorbent material should be placed on the floor to absorb any askarel fluid that still drips from the transformer. c. Place all materials in the appropriate salvage containers during the dismantling for later disoosition. d. All used materials, including rags, sawdust, tape. etc., ngerdiess of quantity, dtouid be put into the appropriate containers for disposition. S. TRANSFORMER DISPOSAL The ultimata disposal of an askarel-lilled transformer may be accomplished in either of two ways. a. Complete drainage end dismantling with the proper disposal of the askarel liquid and askarel-soaked components at described above. ' b. Disposition of askarel transformers by means of junk or scrap daaltrt should be avoided unless t transformer is first drained, followed by soaking of the interior with a suitable solvent, such as kerosene. Accumulated iiouids and washings art to be disposed of as described earlier. IX. Expqctad Service Life Manufacturers indicate that property designed end installed askarel transformers are expected to give trouble-free service for at 'east 30 years. Since their introduction in 1932, the manufacturers report finding the overall failure rate to be less than 0.5% for all units under test and service conditions. The Edison Electric Institute s report (1956-19581 on their member utilities publishes the failure rate for askarel transformers as 0.13 per hundred banks per year. Mr. Frank M. Clark, who inventad transformer askarels st the General Electric Company in the early 1930s, made the highly pertinent comment baaed on his many years of experience with G.E. Pyranol (askarel type) transformers that - .. "The important thing k to *fp them Ory - otherwise leave them Theta words of wisdom became especially applicable in more recent years when welding shut rather then gasketing became the mam method of seeling mkati transformers. These units art sold with the smderatandmg dm the liquid is m a normally harmaticaily closed ayslam. . ... "' > ' k. X. General Characteristics of Transformer Askant Fluid Appreciation of die following characteristics, at given m the IEEE Gtride, leads te understanding die reasons for selecting dielectric breakdown vritags and moistve as tha prime practical tests to judge tee quality of transformer adcarrl fluid. Abo. due to these characteristics tee power factor of transformer askarel will be normally muds higher tewi dw corresponding values for mirwral oil. ' .te mineral inndating oil. mkanl a a relatively polar M; iie., id mteUahm an dipola. fra* to rotate wound their axes pad ratpenete to orientation by dactrieal forces. Askarel also exhibits ' * nMte higher dMactris nmnient and capacitance than insulating oil. -and thaw dffereoraa must be kapt in mind whan intarprating electrical . wetdra. - ` hiflh solvency power, asktrel than mineral oil to traces of polar materials, and eonaaoutndy tee choice of * ^ C8RN 000908 ^ 0 4 LEXOLDMON003192 constructional materials destined for use m adtarel is very critical. This sensitivity is reflected in the power factor and resistivity (specific resistance) of the askarel. It is important to note that, with the exception of water, the dielectric breakdown voltage of askarel is not generally adversely affected by many of the soluble polar materials to which its power factor and rtsistivity (specific resistance) are so sensitive. In fact, the dielectric breakdown voltage of askarel is somewhat greater than that of insulating oil. Therefore, the values assigned these dielectric fluids in newly supplied transformers are X KV min. and 26 KV min., respectively. ,, At with insulating oil. askarel must be kept dry. ft can pidt up moisture from exposure to humid atmosphere. Under similar conditions of exposure, askarel can pick up nearly twice at much moisture when measured on a parts per million weight basis. XI. Sampling Transformer Askarel Fluid The following precautions about sampling ere Quoted from the IEEE Guide. "Representative temples, whether of the complete contents or only pans thereof, are extremely important from the standpoint of evaluation of the quality of the product sampled. Obviously careless sampling procedure or contamination in the sampling equipment will result in a sample that is not truly representative. This generally leads to erroneous conclusions concerning quality and incurs loss of time, effort, and expense involved in securing, transporting, and testing the sample. It is strongly recommended that all of the procedures and precautions outlined in the latest revision of ASTM 0 923 (Sampling Electrical Insulating Liquids) be followed. "Because Of the high specific gravity (relative density) of askarel (greater than II, water and some other impurities are most likely to be found at or near the surface. The top sample, therefore, is considered to represent the worst condition." XII. Evaluation of Askaral Received in New Equipmant Some users of askarel equipment find it desirable to make "at received tests" on ell equipment. It is quite common to use the dielectric breakdown voltage test and visual appearance as the most significant tests. If suitable eauipment end trained personnel are available additional information may be obtained from the power factor, eolor, and moisture content tests. . In sampling askarel contained in apparatus extreme care must be exercised in order to obtain a representative sample. ASTM Method D 923 should be followed. New equipment with asfcarrf exhibiting the following characteristics is considered acceptable: Dielectric Breakdown Voltage Color Condition - Visual Water Content Rower Factor at 2S*C 30 KV min. 300 max. (Strew color) Clear 36 ppm max. * ASTM Methods D 877 D 2129 D 1702 0 1533 D 924,0 160 *The power factor of askaral takan from new transformers, reactors and accessory equipment can reflect the presenoe of moisture, dissolved polar compounds, or other contaminants and may vary with tha type of equipment Worn which the cample was t takan due to the different ratios of liquid-to-solid insulation and to tha high lohaecu power ef tbs askjrsl. Given an ecotptsbie water content and dielectric breakdown voltage of the askarel m i. indicated dMve, a high power factor seldom impairs tha sarvtcertliw the adrjrel within rather broad limits cod is GBRN 000909 LEXOLDMON003193 indicative of the de/M of extraneous soluble polar miter.iis present. Recognizing tfw possibility of e wide range of power factors being recorded for askarel in new equipment, it is difficult to estaDhsn a tingle limit which would be acceptable to both suppliers and users for all applications. However, as a broad guide, power factors up to about 10% at 25* Cand GO cycles per second (hertz) do not in general indicate any abnormal contamination providing that the other criteria (water content, dielectric breakdown voltage, etc > * are met. Much higher power factors may indicate excessive contamination or the misapplication of the solid materials used in manufacture in contact with the askarH and should be investigated. XIII. Dielectric Breakdown Voltage -- Moisture Relationship The dielectric breakdown voltage of askarel is highly sensitive to excess moisture; not sensitive to ordinary dissolved polar materials. White the dielectric breakdown voltage can alto be lowered by severe areng, askarel turns noticeably black or has particles of sooty'carbon floating in it if arcing has occurred. Then the transformer should be repaired and the askarel replaced. If the dielectric breakdown voltage is checked periodically and decreases significantly -- this indicates moisture pick-up, arcing, or both. When die dielectric breakdown voltage has dropped to 26 Kv or lets, an analysis for water it necessary. If water is found in excess of 40 pom at room temperature, its source should be located and corrections male. When the moisture content approaches 125 ppm (saturation level at room temperature), the dielectric breakdown voltage of askarel crops below the value required for efficient insulating. The moisture content should not be allowed to rise over 70 ppm, sampled at operating temperature. If the moisture content it found to be m a satisfactory range and the dielectric breakdown voltage it low, the transformer manufacturer should be consulted. Table IV shows the relationship of dielectric breakdown voltage vs. moisture end Table V indicates the approximate water solubility limits in askarel and mineral oil. TWsle IV Halation of Dielectric Breakdown Voltage to Amount of Disslvad . . Water in Aritarel and Mineral Oil Water Content (PPM) Breakdown Voltage (ASTM DB77! Askarel Mineral Oil 0 : 20 * 40 ao 80 110 70 KV 55 47 40 38 10 50 KV 39 30 26 22 5 IxVv 'Ii^ViVV?r-v li--'.!-- --Iv'--.. 6BRN 000910 LEXOLDMON0031Q4 Table V Approximate Solubility of Water in T reinformer Askarel and Mineral Oil c. F. - Amount of Water (PPM I Dissolved Askarel Mineral Oil -30 -22 20 4 -10 14 0 32 10 50 20 68 30 86 40 104 8 16 26 41 65 94 128 170 8 10 13 20 33 . 58 85 130 XIV. Turbidity ... may be the visual sign of undissolved water, or may indicate dirt. Cloudiness may also result from cold precipitation of tin tetraphenyl "scavenger** that was used in the earlier Pyranol transformers. This scavenger begins to come out of solution around 15*F above aero. To redissolve it requires heating to 150-200*F and agitation. High dielectric breakdown voltage will quickly indicate that any turbidity present is not moisture: that the insulating efficiency of the askarel is still excellent. However, if the dielectric strength is below 26 KV. moisture should be determined, using the Karl Fischer method IASTM 01533-601. The dielectric breakdown noltage test for eskerel serves primarily as an indicator for moisture. It is by far the most important maintenance test for transformer askarel. XV. Check Points for Maintaining Askarel Insulation A. General Considerations: Modern askarel transformers with welded construction or silicone or Viton* gaskets (hand hole-cover, switch and terminal compartment covers) and with properly constructed bushings require little or no maintenance. With properly constructed transformers, annual or semi-annual visual inspection and dielectric breakdown voltage test of the askarel fluid should suffice for routine maintenance checking over many years of service. However, many askarel units were installed in the early 1930s -- before the development of some of the better modem gasketing materials and before improved designs were developed for sealing out moisture. Such early units should be, and can be, modernized. Leaky or deteriorated gaskets should be replaced. If the edcarel has become contaminated, it should be reconditioned. At the same time, a general clean-up of the unit and possible refinishing may be desirable. If it is not convenient to take an old transformer out of service for general repairs, leaky gaskets can be sealed temporarily by painting over the leaky aru with epoxy cement. A survey of users indicates a good number of early-built askarel transformers (over 20 years old) are kept in continuous servica in critical inetadationa by the following steps (instead of modernization). . The operating units are equipped with compound pressure gauges for reading pressure above and below aemotpheric. Positive Trademark of E. I. Di?onc OeWemoun A Creipenr. tee. m CBRN 000911 LEXOLDMON003195 pressure is maintained on the shell by introducing nitrogen it 2 :o 3 pounds itoove atmospheric. Regular workmen m tne irei duty record the tempereture ind pressure. If i sudden pressure drop is noted more nitrogen is introduced end the geskets ere cneeked for leeks with soap solution. Leaks arc sealed by applying epoxy B. Modern Sealing Procedures: Transformer purchasers should specify the following modern techniques for sealing: 1. Welding Construction: Covert, radiator connections, switch and terminal housings, instrument connections, etc. should be welded. - - 2. Bushing Connections; A number of bushings have been developed to obtain a proper seal for the electrical connection through the tank wall. They are classified is follows: II Welded Type (Bushing flange welded to tank will) a. Cast resin bushing with a molded seel to the bushing stud and external stainless steel or copper flanges. b. Rolled flange bushing with the metal to porcelain seal at the cap and flange made by being roiled into grooves in the porcelain over silicone rubber rings. The seal between the cap and stud is made by welding. c. Porcelain or glass bushings with metal to glass or metal to porcelain seals. 2) Bolted Type (Bolted to tank waul ' a. Cast resin bushings with either cast or metal flanges containing recessed gasket grooves, b. Porcelain or glass bushings with flanges containing recessed grooves or gasket stop. . The gaskets may be either of rectangular or circular cross-section, usually 'A inch thick. Bushings with recessed grooves are suitable to use with cork, eork-nitrile rubber combinations or nitrile rubber as well as gasket materials such as silicone or Viton. 3. Small Sire Connections: When not possible to weld, small - size connection seals should be made with Flexitaihc* stainless steel rings. The surfaces must be machined and parallel. The filler between the steel laminations of the Flexitallic ring should be either silioone or Viton. 4. Gaskets for Hand-Hole Covers: Modern design specified silicone gaskets. Such gaskets must be retained in a groove. The groove preferably is machined into the flange or cover. However, it can also be formed by welding concentric steel strips to the flange or the cover. Generally the gaskets should be 5/16 to 1/2 in. thick for covers, depending on the depth of the groove or stop. A rectangular cross-section is usually used. ' The silicone material should be Dow Coming No. 50 Silastic** or equivalent. This is a low compression set material. For best sealing 20-25% compression is recommended, with ample clearance in the groove or stop to allow for this compression. No cement is required. With reasonable care the gasket if removable without damage and is reuseable. Silastic 50 is siightty swelled by askarel which contributes to the tightness of the seal. It is not deteriorated by askarel fluid or vapors. It resists weatherirg and it is thermally stable and 'Trademark of FtextelUc Gartet CavernI, "Trademark of Don Comma GBR* 000912 LEXOLDMONOQ319fi flexible at *11 operating temperatures. It is an excellent moisture barrier. . NOTE: Dow Coming, Midland, Michigan will supply a list of Silartie 50 gasket fabricators to ell transformer manufacturers or users. They will also furnish technical data. See Appendix K: Seals, Properties and Procurements. _- C. The Older Sealing Arrangemenu: The older type gaskets consist of either cork or cork-nitrile rubber combinations or straight nitrile rubber. 1. Cork-Nitrile Combinations: Covers for the mein tank, hand-holes, switch and terminal chambers, relief diaphrams, etc., art held -n place by studs welded to the flange or by bolts. The gaskets are cut with openings and placed over the bolts. Often Shellac (Westinghouse Style No. 11S0419, or General Electric Company's Glyptal* 1276) is used to cement the cork to the flanges. The following is recommended for sealing with the cork -- nitrile rubber combinations: Use Armstrong NC-7S7 cork-nitrile materiel or equivalent. The gasket can be cut from a single sheet or by scarfing strips of the material. A convenient method for joining strips is to make a Keystone Type joint. For this purpose, Westinghouse, Sharon, Pennsylvania, offers their gasket cutter Style No. 328 B614G01, (about $15). The joints -- and also the gasket - should be cemented to the flange, using one of the above cements. Excess cement should not be allowed to reach the interior of the transformer. After installation and bolting, the outside edge of the gasket should be coated thoroughly with epoxy cement to increesa weather resistance. - This epoxy cement it a pasta, to which a curing catalyst is added immediately before use. Typical are: a. Epoxy Patch Kit el-C Hysoi Corporation, Olsen, New York b. Scotches*!** Bam *4 _ Minnesota Mining & Manufacturing Company St. Paul, Minnesota - c. Adhesive A-1 and Activator Type 8 Armstrong Products Company Argonn* Road, Warsaw; Indiana d. Adhesive 9660-1, Synthetics Organic Company, Cleveland, Ohio, used with activator diethylene triamine (Carbide end Carbon Chemical Company) 2. Straight'Nitiila Rubber-Whan auagpn nitrile robber originally used, irworiably the gadeet was recessed in a groove. This was to piereiTt gedtet flow and to protact the malarial egeinst exoewhw comprewion. Atthoutfi this type seal was not cemented, the nitrile rubber gedtet is not reusaeble. Since grooves has* atreatfy bean provided for nitrile rubber tael, Sibrtic 50 can ba easily ajbrtitutad and it ' recommended. This conforms with modem praams. . XVI. Periodic TMd Irapaetion and What Checkpoints Mam On e regular schedule -- at ns. trine, or twelm -month intervals -- make 'TiaUeauwti of General BleetrirCmmai ^Trademark oT aUnneraw HM*s Rhn jieCamaee i A. Visual Inspection: Atksrsl it t dstr, faint-yellow liquid. After long-term ute this color may grtdutlly intensify to li^it brown. The fluid should remain clew and fret from turbidity or cloudiness. Any color change - sodi at to a green, rad or blue cart - indicetei extraction of impurities (color materials) from the solid insulation. If a distinct foreign color pickhip it noted, dieck the complete range of electrical characteristics and notify the transformer maker. Blackening of the askarel may indicate an arcing condition. Other color changes alone are not danger signals since the dielectric breakdown voltage is not likely to be impaired. B. ' Dielectric Breakdown Voltage If the dielectric breakdown voltage has decreased significantly from the last inspection, or if it hes gradually decreased below 26 KV range (at 25*0 - RUN A CHECK FOR MOISTURE. Use ASTM D1633 (Kart Factor Method). The dielectric brtekdown voltage of eskirtl is the major indicator to the operating efficiency of your liquid insulation. Besides the visual inspection tests, dielectric breakdown voltage is the only test neensary to run on a routine basis. Wsll-sesled askarel transformers have service records of 2S to 30 years on the original askarel. XVII. Inspection Checklist 1. If askarel it dear -- even though darkened to light brown, has no sediment or turbidity, ha dielectric breakdown voltage over 26 K V - give it the inspection "OK". If nkertl it doer, but ha foreign color of blue, green, red ... t is "extracting color" from internal matarials. This is not. of itself, in operating hazard when the dielectric breakdown voltage stays i<er 26 KV and moisture remains tow. However, this rare occurrence calls for cheeking into the condition of the interior construction and consulting the transformer maker. However, when sampling tha fluid care should be taken to avoid getting color into the edcard from paint that may be inside or outside of the tamole valve. If die moisture content it found to be above 70 ppm at operating temperature, than templing should be done at more frequent intervals to establish a possible trend, particularly on outdoor installations. If adsersl is dear, but dielectric breakdown voltage drops to 22 or tower KV. and moisture rises over 80 ppm when sampled it operating temperature ... die askarel is ready for simple "refining". If the moisture is near the saturation level (about 125 ppm at room temperature) a thorough inspection should be made for water droplets in tha transformer tank, and even for "gfobuto" of wafer Boating on the askarel surface. If found, the transformer manufacturer should be consulted for reconditioning both the transformer and the fluid. If ideeref ie dark brown to biadt. If Hack pertides of carbon ere seen, and dielectric strength it low... the askarel has been broken down by arcing. It cannot be refined and should be removed and incinerated under proper condition. (See ANSI Committee CIO? report on Um and Ocgsoaaf of Aakand and AtktrtbSooked Manna*. 116 Em44th Stmt. New York, New York 10017). ' . -a If eny of these fhn simple inspection tests appear out of the ordinary or the reUtiorahip between appearance and test values n abnormal, contact your transformer supplier for a complete analysis. .. - Whenever o earepfe is to be shipped to Monsanto, piease follow the directions shown under: "SAMPLING ASKAREL". LEXOLDMONOQ3198 i * i - .'* ' ..y a .i* V. .<! . 4 ;ll XVIII. Contamination in Trantforman Moitcurt, ptrtieulttt matter tnd troed decompotition producu art known to bt itriout contaminating mflutncat on transformer atkartl. The powar factor test normally utad for the detection of contamination in mintrtl oil fitiod transformed is of little utt for this purpose in askarel filled transformers, due to the extreme effect of extraneous soluble polar materials. This increase in powar factor as illustratad in Table VI has no adverse effect on dielectric breakdown voltage. T*leVI Effect of Common Insulation Materials on Powar Factor and Dielectric Strength (Heat Agad 96 Hours in AskarA at 10FC.I . Material Immersed Askarel After Exposure Power Factor, Percent at 60 eye.. 100-C Dielectric Strength 25-C. None (control) Black varnished doth Copper Pressboard Manila paper Phenol formaldehyde resins Shellac Iron Synthetic rubber 1.0 85.0 15 2.0 15 1.6 6.0 5.0 70.0 36 KV 42 40 37 39 41 36 39 39 Similarly, trace containments from commonly used construction materials can lower the volume-resistivity of eskirel, without effecting its dielectric breekdown voltage. This is shown in Table VII. TMe VII Effect of Common Ineulation Materials on Volume Raeistjvity of Aricarei Sample Volume Resistivity x 10* ohm-cm (at KXTC., 500 Volts DC., 0.1" gap) 1. New adcarel before heat aging ____ 2. New eskarel after heat aging 96 hours at 1(XPC 3. After heat aging with 1 sq. inch specimens of: e. Phenolic resin tap changar material b. Paper ... c. Grade A pressboard (tan) - d. Grade A preuboard (gray) a. Grade A presAoard, taminead atrip f. Cotton wrapping . g. Glyptal 1276 cement, cured 48 hrs. at 110*C 2,000 1,900 1.200 750 500 500 400 300 K While trace contamination easily lowers volume resistivity from high levels, it is important to note shat heavy contamination (as whan arced) dots not lower the resistivity below the order of 10* ohm-cm. at 10CTC. The different behavior of adsarel vs. mineral oil in these respects can be summarized as foiiowir ' - High power factor and low volume resistivity in trgngformor mineral oils era commonly regarded as "danger signals" that the oil has deteriorated and broken down chemically or oaeoaafc* moisture is present. u * -. , . . This is NOT TRUE of ^caref liquid ineulation unless the Jistm irtr breakdown voftaga is lose or the raoieture content is high. ;' GBRN 000915 LEXOLDMON003199 Manufacturers of askerel type nansformm point out that <t * quit* wed known that askerel transformers with initial power factor of me askerel fluid in excess of 50% at room temperature and 60 Hz arc giving satisfactory service life. However, there needs to be asurance that doth dielectric breakdown voltage end moisture are at satisfactory levels and do not show adverse trends. XIX. ASTM Method For Invest!gating The Compatibility of Transformer Insulation end Construction Materials in Askarais This method12 uses the change of electrical and/or chemical characteristics of transformer askerel resulting from its controlled exposure to insulation end construction materials, in order to evaluate their immediate major "contamination" effect on the askerel fluid. Delayed or long time contamination affects may not be detected. The method alto utilizes various physical tarn on the insulation and construction materials aftar controlled exposure to the eskaret to determine the compatibility of these materials with transformer askerel. Properly proportioned specimens of the insulation or structural materials are immersed in refined eskertl for 168 hours et 100 * i*C in e forced draft oven. Changes in electrical end chemical properties of the transformer askerel ere compered against a control sample oi the edterel treated in the seme manner, in absence of the test specimens. Dissipation factor (ASTM D 024) mange is one of the criteria used. The aafcarel fluid it refined by absorptive treatment to a dissipation factor level of 0.0S max. et 10CC end 60 Hz end 0.01 max. at 25"C end 60 Hz. Corresponding values of the askarel fluid after heating 168 hours at 10CC in absence of a test specimen ire 0.07S end 0.02 respectively. The maximum dissipation factor lewis suggested for the eskarei after heating in presence of the test specimen art 0.20 at 100"C and 60 Hz and 0.04 et 2S*C and 60 Hz. XX. Refining Askarpl for Roum A. Filtering Through Dry Blotter Paper to Remove Moisture and Extraneous Pertides: Most operators prefer portable refining apparatus, such at a plate press fitted with dolly, available from Sparkler, Mundelein, Illinois or General Electric Company, Pittsfield, Massachusetts; or the earthen cartridge filter type available from Industrial Fitter Corporetion, Lebanon, Indiana. Filter paper liners for the plate press sis available from Carl Schleicher end Schuell Company, Keene. New Hampdiira and manufacturers of filter presses listed above. The filter paper must be dried immediately before use. For best results, spread the paper for maximum surface exposure in s hot air drcsilaiing own and heat it tar 4 to 6 hours at 11CC. Circulate the askard hot (but not over 4CC) through the filter fitted with the dry poser linen. ' After filtration the dielectric breakdown voltage of the askerel mould be 36 KV minimum. ' 1. Precaution*: Filtering mould not be done when the relative humidity exceeds 7S%. 2. Any flexible haem end geskati on (he refining equipment mould be lined with or made of materials met will not be mftanad by contact with askerel fluid. (Materials lined with Si me, Vltoo or Teflon* or flexible metal materials ere so..aDi*J .. - . ;.V. ___ - . .. 2fn presses of puMismiaii by PdTlI.a^ this--Otai. ir.-v--:' *Tiiaivr*aft-LOtPuWdiuewaibCameww.mc. -AGBRN 000916 _i LEXOLDMON003200 T*teVIII Guide to Rato of Daaolvsd Watar Rnwol By Filttring Adcard Through a Paper Pmss Fatses Through Paper Prats Water in Asfcarai PPM 0 115 t 35 2 22 3 18 4 12 5 10 6 10 B. Disposal of Solid Wastes: The ANSI Guide Rita that, "AN Solid wastes which have been saturated with askarel should be dispoMd of by the following procedure: t. The saturated wastes should be placed into leak-proof containers and transported to a supervised dry landfill site meeting Stats requirements. Alternatively, they can be disposed of by incineration in State-approved facilities. 2. Solid absorbents used for spills can be dispeeed of uncontained in the supervised dry landfill site; transport to the site should be in dosed containers. Alternatively, incineration can be used in accordance with par. B (See Section 4 for facilities)." C. Solid Insulation Requiring Drying: If the solid insulation of the transformer requires drying, consult the transformer manufacturer or an apparatus service shop, as in such case oven drying it preferred. D. Earth Treatment for Maximum Improvement of Power Factor and Volume Resistivity: We question whether pumping and filtering die fluid solely to achieve a change in power factor or volume resistivity done is justified in today's ecological climate regarding PCBs. We recommend that in these situations the original transformer manufacturer be contacted. . 1. Procedure: ; The askarel liquid should be relatively dry prior to the following earth filtration. ' ' As a coating on the filter paper surface use finely divided : Attapulgus clay or Fuller's earth dried and activated by heating for 12 hours St 300-350T immediately prior to use. i The amount of earth lead should be 0.1 to 0.2 percent by ! weight on the weight of tha adcarel to be treated. Adcarel ! weight about 12J pounds per gdlon. .... r To deposit the earth evenly, stir one-third of the earth with a smell portion of adcarel in a dean container. Pump the ! mixture through the filter and follow with boo mom ; one-third portions. Than circulate askarel taken from near j the top of tha transformer, peas it warm (net over 56*0 through tha earth-coated filter and lead back through the : bottom transformer outlet. Continue dreuietion until the . fluid it dear and test dtows that (he deetried properties are ' fully restored. - -. - 2. Effect of Earth on Removd of Scavengers -- Only slight and insignificant leat by salective ddorption of ' tin tctrsphanyl and tpoxidet occurs whan askarel is refined jj by treatment with 0.1 to 0.2 percent by weight of earth. To I remove significant amounts of the scavengers requires GBRN C00917 LEXOLDMON003201 ' Table IX Approximate Relationship Showing tha Insignificant Effect of Power Factor and Volume-Resistivity on Dielectric Breakdown Voltaga of Transformer Adcanf Power Factor (60 eve.) ibtrt ------- 55? Voluma Resistivity x 10* ohm-cm (at Breakdown 10DC, 500 Volts Voltage DC. 0,1" asp) 25*C, 0.1" gap 2% 55% 15% 20-25% 40-50% - 0.05% 0.1% 0.7% 2.0% 1500 500 100 80-70 25 36 KV 35 35 35 35 XXI. Cleaning Arced Trantformon If a unit hat eread to that tha ttfcarai it no longer fit for use, a thorough daaning of tha unit it nacawary before refilling with new eskerel iruulation and returning it to eerviee*. Follow thit procedure: A. Drain out all dark, carbon-contaminated adcarel. Arrange to have the eerap fluid incinerated under proper condition. (See ANSI Committee C107 report.) B. Carefully brush carbon deposits from internal parts and insulation, using toft brisde brush making sure that insulation is not damage. C. Flush thoroughly using new aikarel -- not an oil, not a cleaning solvent. D. Flush a second time with freth asfcarei; drain; then fill to the proper level with new eskerel. E. Energize transformer to warm the fluid for 24 to 48 hours; then circulate the adtard throu0t a filter, returning it to the unit filtered and ready for uee. This awuenai that tha came of arcing has teen anaOftfied and corrections mads. Whan severe arcine occurs, naior rmeirs arc usually necessary and the unit rebuilt. This procedure can be mrilied far Htishma out tht rtpoirad utuu. XXII. Sampling AtJcaraJ Taka a sample as does to tha top of tha liquid surfsot as possible. Many large eskerel transformers have a built-in sampling tube near tht surface lor convenient sampling. Than, to make sura that your sample truly nprsaanta your eskerel insulation, take another sample from tha bottom. If additional sampling tuba connections are contrived on tha calves for easier sampling, make die tubes of dean glass, ttainltti steal, aluminum or tin for rigid types; and silicone, or Viton or Teflon tubing for flexible type*. the NEW containers for tht adcarel sample. A new and thoroughly pre-drled, small-mouth quart glass bottle fitted with a Bakeiite* screw op with aluminum or tin cap liner is recommended for quick, on-site tasting. (If complete analysis ie to be made, a 5-pint size sample is required.) . Be sure *>at tha new botde does not stand open to collect duft or moisture. Rinse the temple botde md cap lining two or three times with eakeref from the transformer, then fill it. If the sample will be lasted prompdy. a dear gfass bottle can be used. If sample is to be stored indefinitely, oee an amber bottle or wrap dear glass with aluminum M. .. A. Stieet a dry day. Do net ample intdetion on a warm, moist day whan humidity exceeds 7M, and . CRfiN 000918 LEXOLDMON003202 B. Make sure that the askarel u at least as warm as the surrounding air. (Cold liquids can condense moisture from humid air.) C. When sampling askarel from transformers, it is best to take the sample when the unit is warm and operating at average or maximum load, especially for a check on moisture as reflected by a dielectric breakdown voltage test. Sampling the warm askarel more truly represents its condition during operation. Experience shows that water will migrate from a transformer's solid insulation to the askarel liquid and vice versa, depending on temperature. Therefore, when the transformer is hot, the moisture is most likely to be found m the liquid. This accounts largely for periodic variations m dielectric breakdown voltage. For example, a relatively high dielectric breakdown voltage may be found during winter months and a relatively low dielectric breakdown voltage during the summer months on samples taken from the same unit. When testing has been completed, the remainder of the fluid sample should be destroyed by high temperature incineration described in Section VIII. LEXOLDMON003203 Askarel Filled Switches and Terminal Chambers I. Introduction High voltage lead* art usually connectad to askaral or mineral oil-filled * network transformer* and power centers through terminal chambers and twitches. In tom* cases terminal chambers are not used, and the high voltage leads are connected directly to the twitch terminals. They may be filled with either askarel or mineral oil. Switches are usually rotary or drum type fitted with a revolving block and porcelain unit as the principal element arranged for three-phase service. . Askarel transformers with attached switches haw been in us* for about 30 years. When they were first introduced, the availability of insulating and gasketing materials was rather limited and even the best materials at the time had no service history. As a result, inadequate gasketing materials such at cork, nitrile rubber, and nitrile rubber-end-cork particles were used. While satisfactory for a limited period of time, these materials cannot be depended upon for the expected long life of the equipment. The terminal chamber it usually above or below the switch compertment and separated by a steel wall through which the bushings are inserted. When bushings are' properly selected and correctly installed, there it no leakage from on* compartment to the other. With poor bushing seals, and the terminal chamber above the switch, potting compounds or cable oil can seep into the askarel. When the terminal chamber it below the twitch, askarel can drain into the terminal chamber. II. Sources of Contamination There are three possible sources of eontemination for askarel in switches and terminal chambers: they rank in this order of frequency: (1) water enuring through poor gaskets: (2) decomposition products from arcing when switch is used to break magnetizing current; (31 antrance of pothead or cable compounds through leaky bushing seals. Unlike an askarel transformer where the amount of contaminant it likely to be wry small (probably only traca amounts) in relation to the volume of askarel fluid - in twitches or terminal chambers witn faulty seels, the amount of contamination can be rtlatiwiy large. Experience has shown that, based on the number of installed aakarel-twitch units, the percentage of failures is extremely small. When investigated, it hat been found that most failures originate in the switch chamber. Water is the chief source of contamination. However, heavy contamination of askaral with petrolatum and asphalt material, due to leakage, haw caused a few failures. Petrolatum it used frequently for filling terminal chambers. When either cable oil or petrolatum seeps into askarel, no greet harm results. The fir* resistance will be somewhat decreased and power factor of the askarel will increase with an accompanying drop in resistivity. While highly undesirable, it it doubtful that failure of the unit results. Where asphaltic compounds are used in place of petrolatum, the danger it increased somewhat because asphaltic contamination may cause excessively high dielectric losses in the askarel. When the terminal chamber it below the switch chamber, the potting compound can be contaminated by askarel if the bushing seals are leaky. This is undesirable because the askaral will increase the power factor and conductivity of the porting compound or cable oil and develop heat from dielectric lost. If tfiit mixture is drawn into the cable <*BRN 000920 LEXOLDMON003204 mafetiofc'a cable failure likely. This again emphasizes the iimamma of tight btohing assemblies. III. Sating Switches and Tormina! Chambar* Proper budting eonatruetien, um of Static taalt and welding whartvar posable it highly dnirabla (at cowed in Saction A). Where an elastomeric sail is to ba used in contact with both asfcartl and petrolturn oil, OuPont's Viton is suggested. Far new equipment the user should specify these modern sealing arrangements to keep out contaminants and minimize maintenance. IV. Askaral Utad Under Mild Arcing Conditions Tha IEEE Guide for Transformer Askaret calls attention to tha following: "Askar*! it used, to tome extent, in apparatus where it is subjected to light intermittent arcing, such as in self-contained induction regulators, where operating switches are continually producing slight ares, in transformer de-energizing switches, etc. Under normal conditions, deterioration of the askarel is very slight. However, improperly adjusted or defective switches in this type of apparatus can produce excessive and prolonged arcing and accelerated deterioration of the askarel. It is recommended that when askarel is used under these conditions, checks of the liquid, especially for moisture and dielectric breakdown voltage made more frequently than when it is used only at a cooling and insulating fluid. Deterioration of this type is indicated by a blackening of the liquid. It can usually be reconditioned as previously described. Special attention should be given to maintaining the scavenger at the appropriate concentration." V. Maintenance for Asksrol Filled Switches A. Switches used for grounding after power source has been deenergized will not undergo arcing. B. Switches interrupting magnetizing current will be subject to arcing; the amount of decomposition will depend on power interrupted, time and frequency of operation. As a general rule, the liquid shouldbe checked after S to 10 operations. 1. On newly installed switches, check the askarel at 3.6 and 12 month intervals; if found satisfactory, check once annually thereafter. With prooer attention to die gasketing of covers and bushings, experience will probably indicate that less frequent inspection is warranted. 2. Check askarel for: a. Dielectric breakdown voltage (ASTM 06771: It should be 28 KV minimum. If dielectric breakdown voltage it low. confirm presence of water by Karl Fischer method ASTM 0-1533. Filter to remove moisture. Dielectric strength should then be 30 KV minimum. b. Presence of carbon from arcing: Fluid should be relatively free of carbon. If badly arced and very black, replace fluid. If only minute amounts of carbon are present, filtration is recommended. Check power factor of liquid (should not be over 5% at 25*C and 60 cycles). Flush out switch chamber with several gallons of fresh askarel before refilling. 3. If there is discoloration, high power factor, detectable changa in specific gravity or refractive index, or if fluid flashes below ' 250TF, there is a possibility of seepage of potting compound into the switch compartment. In this cate, correct any leaky bushing seals with proper replacements and fill with new - askarel. 4. * If termind chamber is below switch, cheek potting _ compound for presence of askarel (can usually be detected ' by odor or by an increase in specific gravity). If askarel is present, correct any leaky bushing seals with proper replacements, and renew compounds. - 5, . Essmmp povar gaskets visually. Deterioration can be detected by swelling and cracking of tht npoaad adga. In earn oft* > severe deterioration, liquid seepage it usually present. * TrsT. 6. Chaek far leakage at padring gland of twitching dwft. If7' Jr. leaking, repack with a Silaatic ring type gatkat. ' ''* . VI. Askar*! Under Excaative Temperature or Fault Condition* ' Tha IEEE Guida alto pointt out that. "Chlorobenzenes utad in tramformer atkaralt begin to boil at ttmperaturet of about 205*C, under atmotpharic conditions. If tha material it heated to tuch high temperature in a waled tyttem. pressure develops. Pressure will alto develop in the tyttem if tha atkaral is arced sufficiently to generate copious hydrogen chloride gat. 'Therefore, it is recommended that wherever possible, waled atkarel-filled equipment be provided with pressure relief devices. These devices must be large enough to provide immediate relief at a definite pressure, and to prevent further build up of pressure if decomposition continues. It must be remembered that the presence of devices of this son does not necessarily preclude the rupturing of containing vessels, since pressure build up can be extremely rapid under violent arcing conditions." ' >p v GBRN 000922 LEXOLDMON003206 Transformer uteri not wishing to make thoir own fluid analysts can obtain tha sarviea from Monsanto. Simply contact Monsanto and specify what analyses art wanted. You will be tent tha proper-sizr-: dean sample container, fitted with a proper label. When you receive this, carefully take your temple (following the procec.re for sampling in this guide). Send the container to Monsanto's laboratory. Charges listed indude sample container, shipping, handling and laboratory costs. Typos of Analyses Available Analysis I) - ROUTINE MAINTENANCE CHECK Total Charge: S2S.OO To determine the general condition of the fluid and find whether further analysis is necessary, (one-quart sample required) Properties Tested Dielectric Breakdown Voltage Color and Condition ' Moisture You will ba notified of the results of this test. If further testing is indicated, and you want a complete analysis, you will be sent a five-pint sample container. This sample will be used for the following series of tests: Analysis 2) COMPLETE ANALYSIS Total Charge: $55.00 (1) To determine die extent of fluid contamination, (2) earth refinement to determine what degree of restoration of electrical end insulating properties is passible, (3) check test to see how the fluid responded to earth treatment. a) Complete Analysis: to determine die extent of contamination Properties Tested Color and Condition Free Chlorides Acidity Specific Gravity Dielectric Breakdown Voltage Refractive Index Water Power Factor, Dielectric Constant, and Resistivity b) Earth Refinement Response: Consists of treatment for 2JB hours at 50-6(PC. with 0.1 to 0.2 percent by weight of properly conditioned Attapulgus clay and than filtration through dry filter paper. c) Analysis After Laboratory Earth Refinement: Properties Tested Acidity Refractive Index Dielectric Breakdown Voltage Water Power Factor, Dielectric Constant, and Resistivity Free Chlorides You will be notified of the results of this test series on your sample. Then after refining your entire transformer fluid fill you can cheek on the results by requestingthe following anelysis: Analysis 3)- - : ANALYSIS AFTER EARTH REFINEMOft Total Charge: S35.00 .. .. (This charge will not apply when - - aotfytes 1 and 2 have already been made.) To determinj whether tha andsa tot.of the askare! fill responded to the same extant at the leboratory sample, (five-pint sample required) . Properties Term*/ . 'Free Chlorides Color and CondWoo' V IIT ' ~ Acidity. Refveetive Index. __ - ' - Dielectric Breakdown Voltage - - Watafr' Power Factor. Dielectric Constant, and Resistivity To arrangefor the daecribed above write to the following address: Paul Monsanto Compang . BODNorth LlndBar^tmfc , St.Louit; Missouri 631OT Samploite I ____ . marked for identification'and tent directly to: MontmwrChomiaftompartv* < W. G Khstnmrich taboretorgy Sauget; I Htn0ta822GE^, . -V Attention: R: Ruatar'' 3r._ f i 0009i3 LEXOLDMON003207 APPENDIX A Aikare! Stability and Competition of Are Formed Go: Atkaral insulation is one of the meet inert, chemicaily-stabie heat reeicttfit, non-eorroshie liquids known. It will not break down, oxidize or sludge when exposed to air and high temperature* 150"C. or even somewhat higher. Arcing, however, will break down the compound to liberate seme hydrogen chloride and small amounts of carbon. . APPftOXIMATE COMPOSITION ARC-FORMED OAS FROM TRANSFORMER ASKAREL BLENDS ASTM TYPES D ANDO (INERTEEN 7040 AND PYRANOL A13UU, ROPECTIVILY) Gas carbon monoxide carbon dioxide oxygen inert gases hydrogen chloride (note the tbssnea of phosgene) Amount 04% ~ ' 04%-' ' 04% 14% 974% This are-formed gas from ASTM Type D and Type F transformer adcarels is non-flammable and ncrwombustible. For ell practical purposes, the amount of get liberated from atkaral under a given set of arcingconditions it about 100 cubic centimeters per kilowatt-second. -. APPENDIX B EFFECT OF TEMPERATURE ON DIELECTRIC BREAKDOWN VOLTAGE OP ASKAREL ' ' . ... : '= Dielectric BreakdownVoltage ASTMD877 67 KV 63 57 SS so - so . 48 . 48 . 6BRN 000924 LEXOLDMON003208 memna^ %. * COMPARISON OP THC APPROXIMATE VISCOSITY IN SAYBOLT UNIVERSAL SECONOC OP TRANSFORMER ASKARELS ANO MINERAL OIL TemfcC --20 0 20 40 90 80 100 A13B38-3 1.000 100 70 4S 39 34 30 IOC Minaret Oil 1.000 ISO 86 49 40 34 30 70-30 2A00 196 85 60 40 36 33 APPENDIX E The thermal conductivity valuaa of tranaformer Pyranol A13838-3 at 27% and 58% ara 262 and 2SS x 10* catorin centimeter*-*, degreae centigrade-*, second-*, respectively. Or, approximataly 0.06 BTU par (hr.) (aq. ft.) (*P.) par foot. Thia aama approximation appiiaa to Inartaan 70-30. APPENDIX 0____________________________________________________ .________________________________ Haat Capacity Ovar the tamparatun range of 26* to 126% tha tpadfic haat of tranaformar aakaral <a doaa to QJO ealorin par gram par dagraa. APPENDIX H____________________________________________________________________________________ Coaffieiant of Expanaion Tha avaraga coefficient of axpanalati of tranafdrmaa aakaral ovar tha tamparatura ranga 20 to 100% ia0.0007 ee/ee/%. Ona gallon would irtcraaaa to 1.066 gallowa on haating from 20 to 100%. APPENDIX I Fira Raaiatanaa. . . Aakaral* of variou* eampoaidonai typn ara uaad. Undar arcing condition tha gaaaa produead, while conaitting of predominantly noo-oombuatitole hydrogen chloride can yield varying amounta of combuatibie gaaaa depending upon tha aakaral typet .- InauMon ayatama incorporating than aakaraia and ealiuioaic or other organic metariaft may, whan arced, produce gaaaoua mixturaa which am moderately flammahia. Aa a precaution, auch gaaaa ihould be ramoved from the aakaral by bubbling dry nitrogen through tha aakaral arid fltnhing tha gat apaoa with dry nitrogen before any work it performed on tha apparatus . v.-'-V T. ' . . GSRN 000925 LEXOLDMON003209 APPENDIX J Still. Properties and Proeurament Dow Corning Corporation, Midland, Michigan with Districts at Atlanta. Boston, Chicago. Cleveland, Dallas. Los Angeles, New York City, Washington, D.C. and Toronto has available Bulletin 09-019. August 1962 entitled "Silastic Design Data". This lists the gasket'fabncators throughout the country from whom the "Silastic 50" gasketing can be purchased m sheet, extrusions or molded shapes. Generally. Silastic SO sheet goods are stocked by local die cutters, hence, could be generally purchased locally. Usually small quantities of gaskets are die cut. If larger quantities are needed, tools are made of the same type used to cut other elastomers. ' Where the gasket is extruded for fitting into a machined groove or between gasket stops. Dow Corning advises use of a scarved joint. This joint is then cemented using Dow Coming's Silastic 140 (clear) or their RTV 731 (whitei materials, which air cure. Dow Corning points Out that the local "rubber" fabricators purchase the Silastic 50 in billet form. This is worked on a roll mill in preparation for sheeting or extrusion. Then to obtain the desired physical properties the fabricator must oven cure the Silastic 50 for 24 hours at 480*F. SPECIFICATIONS* ASTM D676 ASTM D412 ASTM D412 ASTM D395 Color Specific Gravity at 77*F Hardness. Shore A. Scale Tensile Strength, psi, mm Elongation, percent, min Compression Set after 22 hrs at 300*F. percent, max White 1 20*0.02 45 to 60 800 250 30 *Att physical properties measured on 0.075 inch thick samples molded 5 minutes at 24CTF, and oven cured 24 hours at 480*F. APPENDIX K___________________________________________________________________________________ Caution Label ' The following or equivalent caution statements should be fixed on all containers of transformer askarels and the transformers themselves: This product contains Polychlorinated Biphenyls (PCBs). Care should be taken to prevent entry into the environment through spills, leakage, use, vaporization, or disposal of liquid or containers. Avoid prolonged breathing of vapors or mists. Avoid contact with eyes or prolonged contact with skin. If skin contact occurs, remove by washing with soap and water. Following eye contact, flush with water. In case of spillage onto clothing, the clothing should be removed as soon as practical, skin washed, and clothing laundered. Monsanto MONSANTO INDUSTRIAL CHEMICALS COMPANY SPECIALTY PRODUCTS GROUP 00 N. LINDBERGH BLVD. ST. LOUIS. MISSOURI B31M The information herein regarding obtaining optimum results from askarv! fluids n vour transformer has been accumulated py Monsanto - ?r over 40 years from me experience of makers and users of askaret transformers jnd >( >s believed will be helpful. Nothing herein shell be construed as applying to ether than askaret mutation Data and maintenance suggestions herein Oo not apoiy to me stner components of me transformer. All operating and maintenance suggestions recommended by me manufacturer jf me transformer incud aiso be carefully followed. Became thae maintenance directions aoply only to tne askarei msuitft'on, Monsanto disclaims any bab>i*ty !* damage to oruuertv .t in,ury to persons arising from transformer operation. GBRH 000926 LEXOLDMON003210 CUSTOMER SERVICE CENTERS - AKRON. OHIO 44313 260 Sprmgtidt Drhrt Morurett OtvtlepmtrU F*rk Til. (216) 666-4111 ATLANTA. GEORGIA 30333 320 Inttrttttt North Ptrkwty Sum 500 Tot. (404) 432-1111 BOSTON, MASSACHUSETTS 02149 Crtrtlt SUtiOh Ttl. (617) 367-5010 CHICAGO. ILLINOIS 3156 On Mtintt Art. On Kltinti. IHinoil 60018 IN. (312) 296-6666 CINCINNATI. OHIO 45236 8041 Holbrook hold Tot (513) 954-1100 DETROIT. MICHIGAN 500 Nerthhnd Town Witt Southfitld. Miehigin 46075 Ttl. (313) 357-0910 HOUSTON. TEXAS 77027 1301 hott Oik Towor 5051 Wttththntr hold . Ttl. (713) 621-9550 LOS ANGELES. CALIFORNIA 90022 6670 6. Mount St TH (213) 723-2492 NEW YORK. NEW YORK 10036 1114AtoutofthtAmtrictt Ttl. (212) 764-5000 ST. LOUIS. MISSOURI 63166 800 N. Undbtrgh Bhrd. Ttl (314) 694-1000 SAN FRANCISCO BAY AREA 2710 Ltftftttt Strut Chrt. CtUforrtm 95062 Ttl. (406) 243-0414 SEATTLE. WASHINGTON 98121 2112 Third Autnut Ttl (206) 622-4203 WILMINGTON. DELAWARE 19810 Suht 204. Btneroit Bldg. 3411 SlhtmdtKotd Ttl (302) 476-4600 Monsanto Industrial Chamicals Co. A Unit of Monsanto Company 800 N. Lindbarph BM., St Louis, Mo. S3166 JV, 'j | K) GBRN 00092? -.3.a LEXOLDMON003211