Document qk2Vg02ywKYQKV9vvjG7vDxz5
STLCOPCB4094902
DISTRIBUTION
File
.
R. E. Hatton
H. K. Nason - File
Duplicate File
Clrc . Assoc, and Assist. Res. Directors fP^t L!
G. R. Buchanan - Org. Development
F. H. Lahgenfeld - Org. Sales
Extra
Extra
Extra
This report contains confidential information which is the
-per-
ty of the Monsanto Chemical Company and which shall be disclosed
only to duly authorized persons. The recipient i3 held accountable
for the filing and safe custody of the report, which must be re
turned on demand.
if 4 (
in I If
,
DSW 620875
*I
STLCOPCB4094903
table of contents
Page No,
I. INTRODUCTION ........................................................................................... 1
II. SUMMARY AND CONCLUSIONS .................................................................. i
III. REFERENCES......................................................................................................1
IV. EXPERIMENTAL WORK AND DISCUSSION . ..... ........................ .... .
A. Evaluation ofC .atomer Samples........................................... 2
1. Skydrol 7000 ............................................................................. 2 2. Pydraul F9.................................................................................. 3, 4 3. Pydraul' 600 ................................................................................4 4. Pydraul 150................................................................................4
B. Study of Fluid Properties ..................................................
1. Flammability of Pydraul F9 via Incinerator Spray Test........................................................................... 5
2. Evaporation Rates of Pydraul F9, Mineral Oil, and Water Base Fluid....................................... 5, 6
3- Pydraul F9 Compatibility......................................... 6
C. Study of Competitive Fluids .............................................
1. Houghto-Safe 271.............................. ......................... c, 7 2. Dasco E36-5OO ...................................................................... 7 3- Cellulube Fluids..................................................................... 7, 8,
V. ACKNOWLEDGMENT......................................................................
9
1
i SW 620876
l
STLCOPCB4094904
-M-?
i|
I t k
I. INTRODUCTION
%
-5 -4
t1
Monsanto's line of functional fluids includes, four products
which are full fledged sales items. Hie3e are Skydrol 7000, a
fire resistant aircraft hydraulic fluid, and Pydrauls F9, 150,
and 600, fire resistant industrial.functional fluids. Customers
using these fluids have raised numerous questions concerning the
fluids and their life and utility under specified conditions. In
attempting to answer such questions, samples of U3ed fluid and
system deposits were evaluated and various fluid properties were
determined. New competitive fire resistant synthetic fluids were
examined to provide data for the sales effort and to keep abreast
of developments in,the general field. These activities have been
labeled sales service work and are detailed in this report.
II. SUMMARY AND CONCLUSIONS
Service was rendered to seven companies on Skydrol 7000 and to twenty-3even companies on the Pydraul series. This service ranged from analysis of a single sample of used fluid to determine re usability through studies of system deposits and components to involved evaluation of Pydraul F9 recovery technics. Data derived from these studies we.re supplied to the customer through the Sales Department for his immediate use in his particular situation. Such activities have helped in securing Monsanto's present posi tion in the field and in the promotion of functional fluids.
Additional properties of Pydraul F9 were determined. These in cluded flammability, evaporation rates, and compatibility.
Several fire resistant industrial functional fluids competi tive to the Pydraul series were examined. Hougto-Safe 271 and Dasco E56-500 were shown to be typical water base fluids. The Cellulube series were found to be essentially triaryl phosphate fluids .
:il. REFERENCES
1. Final Report, "Hydraulic Fluids and Synthetic Lubricants," 117-2030, by R. E. Hatton, May 15, 1952.
2. Final Report, "Functional Fluids-Application Research,
1952-1959", 117-2508, by R. E. Hatton, L. W. Bannister, W. E.
Koerner, 0. B. Cecil, August 9, 1359.
* *
3- Final Report, "Functional Fluids",
Hatton, May 21,,1953-
it k : $ I !'
;U 1 Jt
: .)'* JProgiiesS flf{firths-, j Furicpijojia
117-2330,
by R.
E.
'4jawf J htpJpii il
1 DSW 620877
STLCOPCB4094905
IV. EXPERIMENTAL WORX AND DISCUSSION
? A. Evaluation of Customer Samples
tvr$ : l"
i'r~ As any new functional fluid Is Installed and is used In an
actual mechanical system, certain problems connected with that
particular application arise. Many of these problems are mechani
cal in nature, others are concerned with fluid characteristics.
These latter problems have led to the evaluation of many samples
submitted by our customers through Sales Department personnel.
Such studies are necessary to insure our present position, to pro
mote our present fluids, and to develop new uses fcr present fluids
and leads for new products.
Much of the information obtained on these samples is only of immediate interest to the customer and is of value only to his particular application. Such information has been supplied directly to the customer through the Sales Department and will not be re peated in this report. It is felt that such data are of little permanent value because of the lack of actual details concerning contamination, conditions of use, dilution, etc. and the specifi city of the customer's operating routines and equipment.
A list of the samples evaluated is given in the following tables divided according to the fluid involved. These tables con tain the customer concerned and a reference to the Monsanto per sonnel requesting the work and the date of the request. Information felt to be of future utility obtained in these studies follows each table.
1. Skydrol 7000
Sales service samples of Skydrol 7000 evaluated for customers are listed in Table 1.
TABLE I
Customer
Location
Reference
New York Air Brake Co. United Air Lines Bell Aircraft Corp. New York Air Brake Co. Capital Airlines New York Air Brake Co. Delta-C and S Airlines
Northwest, Alrllxie.4 tifitairfanfeg i c
Watertown, New York
Buffalo, New York Watertown, New York
* Watertown, New York
.Hollir oot
F.H.LangenfeId,6-28-54
F. H.Langer.feld, 12-20-54
H.S.Litzsinger,12-9-54
H.3.Litzsinger,1-18-55
.F.H.Langenfeld,2-14-55
H.S.Litzsinger,2-18-55
F. H. Langenfeld-, 4-25-55
fcF.HJlangenfeld, 5-51-55
Sc'e Sir 5
(
-***:*
' ' ~7
DSW 620878 STLCOPCB4094906
'* V
mm
Pydraul P9
* Sales service samples of Pydraul F9 evaluated for cus tomers are listed in Table II.
TABLE II
Customer
Location
Reference
Cuno Engineering Corp.
J.S.Harris, 11-24-53
Eastern Metal Products
Company
Tuckahoe, N.Y.
Hardy Manufacturing Co. Union City, Ind.
.Geisman, 11-30-53 .Harris, 12-14-55
Aluminum Co.of America Garwood, N.J.
.Geisman, 12-14-53
General Motors-Brown,
Lipe,Chapin Division Syracuse, N.Y.
.Harris
Trlco Products Corp.
Buffalo, N.Y.
.Harris, 3-3-54
Empire Die Casting Co. Cleveland, Ohio
Harris, 4-14-54
General Motors-Brown,
Llpe,Chapin Division Syracuse, N.Y.
.Harris, 4-20-54
Hydraulic Press Mfg.Co. Mount Gilead, Ohio
Harris, 4-26-54
General Electric Co.- _
Lamp Division
Cleveland, Ohio
.Harris, 6-17-54
Trice Products Ccrp.
Buffalo, N.Y.
.Harris, 6-10-54
Canadian General Elec
tric Company
.Harris, 9-13-54
General Motors-
Rc-cnester Prod.Div. Rochester, N.Y.
Harris, 10-1-54
U.S.Steel Co.-
Benjamin Fairless
Works
Morrisville, Pa.
J.S.Harris, 10-22-54
Raclr.e Hydraulics ar.d
Machinery Co.
Racine, Wisconsin J.S.Harris, 10-22-54
Aluminum Co.of America Garwood, N.J.
J.S.Harris, 11-1-54
General Motors Corp.-
Fat r least Division
Malvern, Arkansas F.H.Langenfeld, 2-14-55
Hardy Manufacturing Co. Union City, Ind.
F.H.Langenfeld, 2-15-55
Trlco Products Corp.
Buffalo, N.Y.
F.H.Langenfeld, 2-22-55
Mall Tool Co.
Chlcato, 111.
F.H.Langenfeld, 4-19-55
U.S Steel Corp. -
Fairless Hills, Pa. F.H.Langenfeld, 4-19-55
Coulter Mfg. Co.
F.H.Langenfeld, 5-11-55
Bendix Aviation-
Scintilla Magneto
Division
Sidney, N.Y.
F.H.Langenfeld, 6-20-'
Alloy Die Casting Cc. Los Angeles, Calif F.H.Langenfeld, 8-23-!
Kitchen Quip, Inc
Waterloo, Ind.
M.C,Plummer, 9-fi~55
Lvupinumii Ccj.. oT*America
,, Ohio
ienfelf 0.C
'SOE
.? Mot
fell
ling
tell
DSW 620879 STLCOPCB4094907
-y v
H ; ? tm
; Afresin banded felt filter was submitted by the Cuno Engineering Corp. for evaluation.' The Cuno filter cartridge No-:. 2278-Cl was received and a portion placed in Pydraul F9 .on Novem ber 24, 1953* The beaker containing this combination was allowed to stand at room temperature until December 14, 1953- The car tridge was removed end allowed to drain. By qualitative observa tions only, it appeared that the filter was not softened. Pelt fibers did not separate from the cartridge. These data do not indicate that such a filter would operate satisfactorily with Pydraul F9 but that the resin bond is not dissolved by the Pydraul
P9
3. Pydraul 600
Sales service samples of Pydraul 600 evaluated for customers are listed in Table III.
TABLE III
Customer
Location
Reference
Aluminum Co.of America
Chapman Hydraulic Press
Machinery
Bellwood, 111.
J.S.Harris, 12-22-54 F.H.Langenfeld, 3-21-55
Los Angeles,Calif. C.W.Fetzner, 10-28-55
A bottle of Pydraul 600 from Alcoa, Bellwood, Illinois, via HPM was received and examined. This bottle was claimed to .-.ave been filled with foam from an HPM machine using Pydraul 600. The gas above the liquid was examined to determine, if possible, whether the gas causing the foaming Is air entering the system through leaks or nitrogen from the accumulators.
Part of the ga3 was displaced from the bottle with water. Analysis indicated that the oxygen to nitrogen ratio was 1. C to 4.1 corresponding to 19-5$ oxygen and 30.k% nitrogen. 7his would indicate that the gas over the Pydraul 600 was essendaily air and the foam problem was due mainly to air entrainment.
4. Pydraul 150
Several samples of Pydraul 150 were evaluated for the
customer listed!ini-Table IV.
';
TABLE IV
istsoma
xfatioh
ice
fK
n "h 1
DSW 620880
I- :
T'~ r! 1
STLCOPCB4094908
Page 5
B. Study of Fluid Properties
1. Flammability of Pydraul F9 via Incinerator Spray Test
The behavior of Pydraul F9 on spraying into open Ilames in an Incinerator was examined. This work was done to provide data for insurance personnel as requested by the Sales Department.
A spray outfit was assembled from materials supplied by Douglas Aircraft Co. The equipment was designed so that nitro gen pressure could be placed upon a reservoir containing the fluid under test and the fluid forced through a small orfice and formed into a fine spray. The pressure used in the tests was 1000 psl. The fluid was drawn up into the reservoir by the use of a suction pump. This equipment was set up in front of the plant incinerator in which a wood fire had been built and after the entire incinerator had become hot because of the burning of waste paper. Temperatures of 1100 to 14008F. were measured in the incinerator by means of optical pyrometry.
Three fluids were used, Pydraul F9, DTE Medium (mineral oil), and Houghto-Safe 271 (water base fluid). Spraying the DTE Medium into the Incinerator resulted in vigorous burning as the fluid contacted the flames and hot surfaces. Spraying Pydraul F9 tended to increase the flames slightly, the fluid vaporizing and burning. There was no flash back. Spraying Houghto-Safe 271 re sulted in no increase in flames. These results demonstrate Pydraul F9's fire resistant properties under the test conditions. The good results obtained on the water base fluid Indicate the effec tiveness of water as a snuffer when the entire fluid is vaporized. Pydraul F9 was decidedly better than the mineral oil.
2. Evaporation Rates of Pydraul F9, Mineral Oil, and Water Base Fluid
The relative evaporation of several fluids was deter
mined in response to a Sales Department request. The procedure
used is as follows: 250 ml. beakers were filled approximately
3/4 full with the fluid under study weighed, covered with ribbed
type watch glasses, and allowed to stand in the laboratory at
room temperature. The fluids examined were Pydraul F9, DTE Medium
(mineral oil) and Houghto-Safe 271 (water base fluid). A similar
volume was used in each case, being about 180-190 ml. The fluid
weights, were about 230, 160, and
grams, respectively.. The
Ibe periodical Iyfan|l> the weight losses obser^fedi >
It
m
DSW 620881
STLCOPCB4094909
fcuffS
?dium~ m Hought
0.0 sw* * 25.3. 50.1 69.6 8o.4
These data show that the Pydraul P9 and the mineral oil, DTE Medium have lost no appreciable amount while the water base fluid, Houghto-Safe 271, has lost about 40$ by weight in 65 days. Both Pydraul F9 and DTE Medium were unchanged in appear ance. The Houghto-Safe 271 sample decreased greatly in volume and the solids which are normally present seemed to.increase slightly in amount. These data point up the problems involved in maintaining the proper concentration of water in water base
fluids and the greater permanence of Pydraul F9. .
3. Pydraul F9 Compatibility
Compatibility data were determined for Pydraul F9. Mixtures of 50:50, Pydraul F9:benzene and Pydraul F9:hexane were prepared. Both mixtures were completely miscible at room temperature and at 0?C.
C. Study of Competitive Fluids
1. Houghto-Safe 271
A fire resistant hydraulic fluid competitive with Pydraul F9 was introduced by the E. F. Houghton Co. A partial analysis was carried out in the following manner.
A sample was fractionated under reduced pressure. The first fraction consisted of water, accounting for approximately 5056 of the composition. The second fraction obtained accounted for about 25$ of the composition and was subsequently identified as dipropylene glycol. The remaining 25$ of the material was left as residue. No analyses were performed on the residue.
The results of the analyses performed on the glycol
fraction are given in the following table along with values for
dipropylene glycol.
Material
1
Specific) *
Boiling
Property
Refractive Point
Gravity
Index
(atmos) $ Carbon j $ Hydrogen
I hi
H l i'
t
m DSW 620882 STLCOPCB4094910
$4* Page 7
These results show that the fraction in question was slightly contaminated dipropylene glycol, 'nils fraction was odorous also indicating contamination. No analyses were carried out on the residue from the distillation.
Physical properties were determined for Houghto-Safe 271. The data are as follows:
Viscosity,
210F. 170F. 130F. 100F.
77F. 68F. 50 F. 25F.
Sp. Gr. 25/25C.
8.56 cs. 13.46 cs. 24.10 cs. 41.9 cs. 70.4 cs. 88.3 cs. 149.4 cs. 575 cs.
Flash Point
28oF.
Fire Point
28oF.
Pour Point
+ 5F.
2. Pasco E56-500
Another fire resistant fluid is Pasco E36-500, a water base fluid. Our sample contained large amounts of sediment. After filtration, the viscosity was 6b.3 cs. at 100F.; separation occurred at 210F. The Dasco was completely soluble in water,
slightly soluble in benzene with separation occurring if larger amounts of benzene were used. The material does not behave like Ucon 200 in this respect; Ucon 200 being not miscible with benzene.
. A flash and fire point determination was run on Dasco E36-500. The fluid boiled vigorously at 210F. and the temperature
stabilized until about half the volume remained. The temperature then invreased .slowly with some boiling. The flash point was found to be 260F. and the fire point 290F. Thi3 is the usual behavior for water base fluids.
3. Cellulube Fluids
The Celanese Corporation of America introduced a series
;ach < w|
1 iI? DSW 620883
s
ifUfrn.M iWn
STLCOPCB4094911
mm
Sample
&S
Cellulube X-90 Cellulube 150 Cellulube 220
Viscosity, 210*F.
3.26 cs.
Viscosity, 100'F.
17.30 cs.
Viscosity, 20F.
420 cs.
Viscosity Index f
+ 35
Acidity
0.04 N.N.
Specific Gravity,25/25C. 1.2059
Refractive Index, 25C. 1.5602
Flash Point
410F.
Fire Point
-.620 F
Pour Point
-40F.
4.43 cs.
35.23 cs.
,3130
cs.
- 31
0.05 N.N.
1.1624
1.5546
450F.
640F.
-15F.
5.04 cs.
49.16 cs.
867b
cs.
- 45 0.04 N.N.
1.1449
1.5518 440F.
65P. -10F.
None of these fluids contain chlorine as indicated by the copper-flame test. Based upon the physical properties, it appears that these are principally triaryl phosphates. Celluflex 150 appears to be a perfect match for tricresyl phosphate. Cellu
flex X-90 is very similar in properties to cresyl diphenyl phos phate (Santlcizer 140 or Celluflex 112). It should be possible to prepare a triaryl phosphate similar to Cellulube 220 by proper selection of the cre3ylic acid used.
The data obtained thus far do not unequivocally identi fy these products but certainly all evidence does indicate triaryl phosphate variations.
The composition of Cellulube 220 was elucidated by
studying the type of cresylic acid derivable by hydrolysis of the ester.
A sample of Cellulube 220 wa3 hydrolyzed by potassium hydroxide and the cresylic acid then Isolated. Distillation of the cresylic acid through a 50 plate column gave the following information as reported by the Analytical Laboratory:
: 2/6 phenol and o - cresol 25# meta and para eresols 39 low boiling (less than 215C) xylenols
- Balance high boiling (more than 215C) xylenols and other high boilers.
This information Is based on boiling points.
The phosphorus content of this sample of Cellulube 220 was 7*5/6.
v i i J i i Hi-1 isd | 5 I jtTrlaryl ptyop]
'`Y.ai fcri Nbsyii'C:
m
.
B^l
DSW 620884 STLCOPCB4094912
>^'-f, 1 -'3K>
..it
- ^y<J **:.
|> %
f Another Cellulube i3 2015 which was reported to be
under test by the Navy. A second sample of Cellulube 150 (Lot
13-54-21) was obtained. Properties of these two samples are as follows:
Sample
Cellulube 2013
Cellulube 130
Viscosity,cs.,210F. 100P. 20P.
Viscosity Index
Acidity, NN Specific Gravity,25/25C. Refractive Index at 25C. Flash Point, P. Fire Point, F. Pour Point, F.
5-07
50.64 9230 -51
0.06 1.1453 1.5517 460 650
+5
4.25
32.31 -----------------
0.09 ----------------455 635 -20
The Cellulube 2013 seems quite similar to Cellulube 220.
V. ACKNOWLEDGMENT
The analyses performed by the members of the J. F. Queeny Plant Analytical Laboratory are gratefully acknowledged.
md 4-20-56
R. E. Hatton
fe:
DSW 620885
STLCOPCB4094913
pf *
1 * rf Wmi^f
Louis earch Report No .lh.523^* '* . - M'S-
May 24, 1956
PINAL REPORTS ON
EXPLORATORY PLASTICIZER AND STABILIZER EVALUATION WORK FOR THE PHOSPHATE DIVISION
J.ob No. 2-02-750.01-2595 AND
SALES SERVICE WORK FOR PHOSPHATE DIVISION Job No. 2-02-750.01-2563
? ' *<$"# *
! t
#* # rf $ ' * i < $
v-i
5T 3 ; /.: .
t, ...
Work done; by.:
MonsantojChemical Company Organic Chemicals Division St. Louis Research Department
kUi | J
i : f f ( i l: : t | >rted by:'
It
; A? 1 ? J 1 111 I H ! > 11 I -1 : I 4 4 I : -t s I .( 4
' f 1 I# g
DSW 620886
STLCOPCB4094914
a ;ji 1; v
* 11
ii
: $' ;i
&
STRI B"U T I 0 N
%
-? * 1. File
S:-
i? t ' >
' *:
2. J. R. Darby
5. J. H. Lum - F. B. Zienty - File
4. Duplicate File 5. Circ. Assoc and Assist. Research Directors Ret ^ Y f
6. L. R. Wangler
7. G. R. Buchanan
8. H. I. Armstrong
9. Plastics
LO. Dayton
1.1. Extra
'B&ra**** '
"
*"**<***- *'
This report contains^ confidential information which is the property
of the Monsanto Chemical Company and which shall be disclosed only
to duly authorized persons. The recipient is held accountable for
the filing and safe custody of the report which must be returned
. ;on ii de. ms as-nd &| t i` J& . #i -*| *f ff-c .- *?; > t. | f
| ; j S , i. ;
*
If l-M -
*
.ii
...
DSW 620887 STLCOPCB4094915
si | - ' 1 I*
it i ; *' s i * % <**
TABLE OF CONTENTS si - * ' # - . :&
Page No.
I. INTRODUCTION..................................................................................................... .1
II. SUMMARY........................................................................................................................1
III. CONCLUSIONS ...................................................................................................... 2
IV. PATENT STATUS..................................................... ............................................2
V. EXPERIMENTAL PROCEDURES...............................................................................5
VI." DETAILS................................................................................................
..... .
A. Application Work onPresent Products........................................ 3
1. Stabilization of HB-40........................................................... 3,4 2. Stabilization of Aroclors .................................................. 4,5 3. Intensive evaluation ofPanaflex BN-1 ....................... 5
B. Technical Service Work........................................ ............................ 5,6
f f C. # Exploratory Stabilizers.. . ..................................................... 7,8,9, ' 10,11
D. HB-40 Substitutes ................................................................................ 12,13, 14
VII. APPENDIX..................................................................................................................14
}.
iI
*' I
? f: H f
I H t'I
i .Jr
DSW 620888
STLCOPCB4094916
, |4^the pas^t^p,;
r ;hat rperioa fof'timel covered by
tha k'tio 13 ob number'll
this (report)', there" hasv existed
a wnrtrlng wlafelonM __
Research and the|old Phosphate *
Division, similar W
1effect between Research and the
Plasticizer Sales Dept". * TOe?
Job numbers concomitant with this
report have been combined
effort to conveniently assimilate
the work that was the outcome|of. this working relationship
t-
All work included in this?report was concerned primarily with
either Improving customer relations or supplying the Phosphate
Division Sales force with graphic information displaying the merits
of their products and/or the possible shortcomings of competitive
materials.
Some of the information contained herein is the result of work done at the request of specific customers, while other facts were garnered in recognition of their being informative to the trade as a whole.
Other work in this report concerns application work on current (at that time) Phosphate Division products, and the screening of -- new products, potentials for exploitation in either the plasticizer, stabilizer, or other, related fields.
II. SUMMARY
The nature of the work contained in this report was necessarily
diverse, being gleaned, as it was, from two separate Job numbers
of varied scope.
_
Three general ;cia3slfdattpns|of|work will suffice to cate
gorize a summary of the information recorded herein. The first
consideration was directed toward application work on present
products, which entailed the ^intensive study of the stabilization
of HB-40 and the Aroclors. New stabilization systems were ini
tiated, and old systems were revised in an effort to achieve
improved stabilization of these products. Intensive evaluations
of a highly competitiveiprodu&t,! Panaflex BN-1,,was also included
in this work.
f ' 'Hl'I'f -
Technical 'service for specific customers of the Phosphate
Division formed thef>sec'orid|prfa.se of this work. -This section dealt
o_ nly jWlth. prob lem3 whJich*- *-weird|s\i>mitted by specific customers .for a paiftlep3.aif evalv|axionfart' CnMrf ? * f M t f 1 t ? I M l ' I ; *
li
HI IM
'.
1 i;
r iliation$ ofI new * exploratory products, j
Lne
tH
DSW 620889
STLCOPCB4094917
cor 3I0NS;
< ft
m.t *, .
I-
of
the "'work described
in
this* repox
K.tt.
0:the'fo*lowing
conclusions were found to be substantiated by experimental proce
dure:
"-
"?
Several organophosphorous compounds impart anV excellent degree of stabilizing power to PVC formulations exposed to ultraviolet light. They were found to prolong stabilization action, in many cases, beyond the excellent period of 1000 hrs. exposure, when incorporated into current stabilization systems or mutations of those systems. The most promising synergistic light-stabilizing action was displayed by:
Tris (9,10 epoxyoctadecyl) phosphite 9,10 Epoxyoctadecyl dlisopropyl phosphite Bis (9,10 epoxyoctadecyl) benzene phosphonate Bis (9,10 epoxyoctadecyl) benzene pho3phonlte Bis (9,10 epoxyoctadecyl) methane phosphonate
Formulation combinations of phosphonates and epoxy alcohol
approach, but do not quite achieve, the stabilizing effectiveness of epoxyphosphonates
HB-20 (T-2, slightly hydrogenated) was seen to be of potential importance as the ultimate choice as a replacement for HB-40.
The organophosphorous compounds which displayed such promising stability to ultra-violet, have little value with respect to resis ting heat degradation. They are poor heat stabilizers^ per se and impart no %ynergistic effect in stabilizer combinations.
V-
Panaflex BN-1 (Pan American Chem) is much superior to HB-20 and
HB-40 in a consideration of volatility. Heat and light stability
tests, however, fail to determine any superiority of this product
over HB-20 and HB-40.
Aroclors 1254 and 1260 achieve their best stability when stabilized with Paraplex G-60, Pyphos, and Mark XV.
- -- _
V
IV. PATENT* SITUATION
,-
5
matloTonnh?pd?ees^carvibee|dbeeinn,
several patent applications* $i&e Using this'report. However, the ch'eemmifs,.ts w.h.o
Slnfor_s_u_b__mit
I 1
the prospective plasticizers or stabilizers thoroughly^cover the
sitldns 4 iMfcic&'&idh j i
II
DSW 620890 STLCOPCB4094918
teat ^thodat uoed ln thiajrepprfclu^^oiwalned In the
revised ,$ comprehensive supplement entitled, Standard*Test Methods,
Plasticizer Applications Lab. .
.
v -. v & 'f;.s > t
This supplement contains essentially all .of^the test methods
used.dLn the Plasticizer Applications -Laboratory*! and will be en
larged as the need for new or more expansive methods of testing
arise.
\
VI. DETAILS
:
A. Application Work on Present Products
iIn the course of this work there have been requests emanating from the Phosphate Division for application work concerning several of the products produced by, and/or of considerable interest to the Phosphate Division. Work of this nature enabled that Depart ment to maintain a cognizance of advancements, technical and commercial, in the field and potential market-improving changes for Monsanto products.
1. Stabilization of HB-40
Heat and light stability screening tests were carried out on thirteen variously-stabilized HB-40 samples in standard formulations of HB-40 (stabilized), DOP, and polyvinyl chloride.
The stabilized HB-40 samples were ider^iMed as follows:
M-II80
M-1181
'HBII-40
stabilized
with
o-tolylblguanide ' cadmium dlbutyldithiocarbamate
M-1182
M-H83
cadmium di-lso-propyldithiophosphonate phenyl arsonic acid
M-1184
M-H85
l,l-dicyclohexyl-2-phenyl urea tin salt of diethyl dithiocarbamate
M-1186 l;
f f .-bis-(l-piperldyl>i^hi6ckrbonyl) dl
' sulfide
' $'
M-1187
N-( 2-hydroxy-3-_n_-butoxypropyl)
ethylene diaminpf ' " '
M-1188, M-II89}
butasan
- ftgf"
A, 3-dlmorpholinppi
it I
t |trlphenyi stitfinef
; f phite
"
M-119l|
trlphenyl stibir
M-II92
* * ` * *-li`
5i
DSW 620891
STLCOPCB4094919
#1
fI f i Heat tests showed roost of the above, formulations ftofbe \
decidedly Inferior, even to unstabilized HB-40. Only two, those . a
stabilized with triphenyl*stibine-tributyl phosphite, and with tri
phenyl stibine, were equivalent, but not superior to HB-40 tihsta-
bilized.
Light stability tests were carried to completion at
I
400hrs. ultraviolet exposure. After this time it was apparent that the stabilizer-HB-40 combinations possessed little or no apparent favorable effect, concerning heat or light stability.
2. Stabilization of Aroclors
a. In an effort to determine the best stabilizer system for use with Aroclors 1254 and 1260, formulations containing these Aroclors and DOP were stabilized using the following methods:
(1)
Paraplex G-60 Mark XI (barium cadmium laurate) Mark XX (triphenyl phosphite)
(2)
Paraplex G-60 (Epoxldlzed soy bean oil)
Oyphos (dibasic lead phosphite) Mark XV (cadmium phosphite)
(3)
Paraplex G-6o Plumb-O-Sil C (lead silicate) DS-207 (lead stearate)
" (These formulations were prepared with both Opalon 500 and Vinylite' * VYNW)
Stability results show that the Aroclor compositions
achieved slightly superior stability when used with Opalon 300, rather than VYNW resin.
The stabilization system consisting of Paraplex G-60,
Oyphos, and Mark XV afforded the best heat and light stability (of
systems tested) to compounds containing Aroclors 1254 and 1260.
The epoxy-cadmium system was nearly equivalent to the aforementioned
| system. Heat stability displayed by these Aroclors wa3 excellent, v ,
| but |th^ light stability .t^e same-compounds'was ?poor. | ; 1 l| ||
tl
;v j
b. Perrot Chemical Co. reported that DOP-Aroclor mlx-
tures show essentially*t aame|^ab^l ty a^D^^|alone , iln ,
"
impl
DSW 620892
STLCOPCB4094920
.......... ^ t ft# ? < - ** # # Contrai^STOlPerroT! a results;lit was ^determined that
the light stability*; iaaoticeablytinferlor ini the mixtures of
Aroclor and DOP, asv compared to DOP, alone. '
3* Evaluation of Panaflex BN-1
Panaflex BN-l^a hlgh-boillng hydrocarbon oil from Pan
American Chemicals, Is a competitive product of HB-40 and HB-20 by virtue of Its lower price, lower volatility, and its supposedly Improved light stability over HB-40 and HB-20.
The following are the results of the activated carbon volatility tests at 87C. on films containing DOP and various concentrations of HB-20 and Panaflex BN-1:
HB-20
Panaflex BN-1
Plastlcizer( PHR)
R5F HB-20
Volatility
Plasticizer (PHR)
DOP Panaflex BN-1
Volatility
50 0 40 10
35 15 25 25 20 30
15 35 10 40
0 50
4.8*
17.3 20.4 24.1 22.8 18.7 16.5
11-3
50 0 40 10
35 15 25 25 20 30
15 35 10 40
0 50
4.8*
13.2 13.8
13-7 12.0
11.7 9.0 2.6
Heat and light "stabilities of`Panaflex BN-1 were deter mined on films containing 25 PHR DOP and 25 PHR Panaflex BN-1, with the epoxy-cadmium stabilizing system. Its light stability is as poor as that found in films containing HB-20. Panaflex BN-1 also induces yellowing in a relatively short exposure time. Its heat stability was perhaps a little inferior to that of HB-20.
B. r Technical Service for Specific Customers
|* if '
Frequently the situation arises where a customer is con
fronted with a'problem concerning the use of one or more of our products in his particular field of production and requests technical service ^toward 4the solving,o.f|that problem. ; Work`done : | g. in feoi^urfctio^ with^|Kese* re*que*sts Us Iconsidered "Sales Service1' anndd'wwaas peerrffoorrmmeeddi'innffoorrdder to imnprove -customer .relations.
I
|* l s
DSW 620893 STLCOPCB4094921
'I *
4
f i
f
fblends used in extruding clothes-line wereI evaluated for physical properties for U. S. Equipment. Both com
pounds contained HB-40 and Aroclor 1254. Both had fairly good low temperature properties but were very volatile. Yellowing was evident on exposure to ultraviolet.
Formulations:
II
Opalon 300 Dicapryl Phthalate HB-40 Aroclor 1254 Paraplex Q-60 Atomlte Mark XI Mark XX Acrawax Titanox RA
Properties:
II
Tensile strength Shore Hardness ` Low Temp. Flex. Volatility Light Stability (Weatherometer)
100 hrs. 200 hrs.
300 hrs.
2156 psl 33 -26. VC.
24.5*
1888 psi
73 -36.7C. 26.o
SI. yellowing Increased
yellowing Same
Yellowed Yellowed
Same r
b. Samples of clothesline from U.S. Equipment Co. containing dicapryl phthalate, HB-40, and Aroclor 1254 displayed excellent stability in both Fadeoraeter and Weatherometer.
2. Western-Textile
The Western Textile Co. requested shore hardne33 data
on resins containing DOP, HB-20, and Aroclor 1254. The following
formulation was-found to meet the shore hardness of 85 desired by
the customer:
,
1 * i I Opaiorf sici I $
- dop H f I ! Aroclor 1254
i| *
If
I1
DSW 620894 STLCOPCB4094922
* f.
.. Exploratory'Stabilizers
.
>* . r
:V .4 ~ : ; f. -. ; ;
...
s 4 r-
Ten exploratory stabilizers were^evaluated under this Job
number, during this period; all were submitted from Anniston. '
In evaluating exploratory compounds as potential stabilizers it
is usual to test them both as primary stabilizers and in combina
tion with several accepted stabilizing systems. This increases
the possibility of observing any stabilizing action inherent
In the product.
Following is a list of the stabilizers evaluated, with the
evaluation results:
M-1526 M-I527 M-I528 M-1529
M-2043 M-2044 M-2045 M-2046 M-2047
Bis (9,10-epoxyoctadecyl) benzene phosphonate Bis (9,10-epoxyoctadecyl) benzene phosphonlte Bis (9,10-epoxyoctadecyl) methane phosphonate
Trls (9,10-epoxyoctadecyl) phosphite 9,10-Epoxyoctadecyl dllsopropyl phosphite
Bis (beta-chloroethyl)ethylenephosphonate Dibutyl allylphosphonate Bis (2-butyloctyl) phosphite
Bis ( 2-octyl)-2-ethylhexanephosphonate
Bis (beta-chloroethyl) beta-chloroethane phosphonate
These ten compounds were Incorporated into DOP-plastlclzed
PVC, alone, with epoxldized oleyl alcohol, with Mark XI, and with
Mark Xj. and Paraplex 0-60. The testing of the combinations of
phosphonates and epoxy alcohol was an effort to approach the
stabilizing effectiveness of previously tested epoxyphosphonates,
with a system which might be economically more practical and
patentable.
... * ^
. :;
Heat tests consisted of sample exposure in a 170C. cir culating air oven with samples removed at 20 minute exposure intervals.
1. Heat Test Results
Generally speaking, heat stability tests indicated the organophosphorous compounds to be of little value in obtaining a synergistic effect. They are poor stabilizers, alone, and only fair when included in stabilizer systems. M-1526, M-1527, M-1528, and M-1529 were essentially equivalent to .each othe^ anti, to the, control in the Mark *XI-G-6of system; but werefleIs* efficient with the removal of Paraplex G-60.
. 9, la epoxycnctadecy^ erfori to t ^eJafdrlmehtllDfec
Lis.ompro
U
IV
DSW 620895
STLCOPCB4094923
!<- Ir-i I
uS
Pr f f;
Bis (Iteta-chloroethyl) ethylenephoaphonate (M-2043)
and dlbutyl allylphosphonate(M-2044),`in combination with 0-60 and
Mark XI dlsplayed^somewhat better* heat-stability than the control
sample-. ; . . ,............'....*...... ;
- . Ii.t ... -
; .
- * .. v _ . ,' .
. ,-
.
Bis (2-butyloctyl) phosphite (M-204_5), bis (2-octyl)-2-
ethylhexanephosphonate (M-2046), and bis ((bbeeta-chloroethyl)` beta-
chloroethane phosphonate (M-2047) were seen to be poor heat sta
bilizers in relation to current stabilization systems.
2. Light Test Results
The ten organophosphorous compounds gave results of interest in that exceptional long-term light stability was displayed by several of the compounds.
Bis (9,10 epoxyoctadecyl) benzene phosphonate (M-1526)
and bis (9,10 epoxyoctadecyl) benzene pnosphonlte (M-1527) showed
excellent stabilizing effects with G-60 and Mark XI for 1000 hrs.
exposure. The stabilizing effects were, however, induced upon the
removal of some of the G-60.
---
Bis (9,10 epoxyoctadecyl) methane phosphonate (M-1528) resisted sample breakdown for more than 1000 hrs. when incorporated into the epoxy-cadmium system.
Tris (9,10 epoxyoctadecyl) phosphite (M-1529) was seen to possess excellent stabilizing action, not only in combination with G-60 and Mark XI, but also with Mark XI, alone. This situa
tion was unique in this series of stabilization studies. Extended exposure to ultraviolet resulted in a remarkable resistance to . breakdown for 1400 hours, a much eater stabilizing effect than displayed by standard stabilizer systems.
9,10 epoxyoctadecyl dilsopropyl phosphite Imparted a slightly more stabilizing effect to the epoxy cadmium system, but showed less interesting properties when its concentration was in
creased, or when the concentration of Paraplex G-60 was decreased.
Samples M-2043 through M-2047 were slightly less effec tive in apparent light stabilizing action than the five samples reported above. |
) | i ? l i -The fee J^iilhtl stability! was! displayed by the-s`erle35 '
containing G-60 andf Mark XI, with"; all five (M-2043 thru M-2047)
possessing very goqd;long-term stability. Both bis (beta-chloro7
hyl), el jylene
is i(k2itutyloctyl)t phos4 i *
it " '
DSW 620896 > s]
STLCOPCB4094924
MyppJPQty1 Jgy^^^lnejcaiwlaMi^bhor
p*8** - ^yner^S^pteffeet TwhfrTused *witfi Mni^ieX fb-6o^ ^r&tRer ____
epoxidize<f oleyl alcohol, while the pother samples showed, results
to be equal, between 0-60 and the epoxy;'alcohol .< i } tS
'i * -- .
%.<
# '
When used alone, these five organophosphorous*compounds
were 3hown to possess poor stabilizing qualities. ; * k -
Formulations used In this work are as follows: 1
SERIES "A"
9,10 Epoxy-
oc tadecyl
Opalon
D1 Isopropyl
300 POP M-1526 M-1527 M-I528 M-1529 Phos
Mark XI G-60
47
190.
1121..
.13.
14. 15. 16 17.
1-5 1.5 1.5 1.5V
fr t
1-5 1-5 1-5 1.5
18.
19.
SERIES "B"
Opalon 300
DOP
M-204^
M-2044
M-2045
M-2056
M-2047
Epoxy
Oleyl Ale.
|f Mark =XI
G-60
100
I
DSW 620897 STLCOPCB4094925
3 a;-
I * #;*# \r %'
|vt !
-i'i-k. &
c'-
Epoxy 4 l m Oleyl 1
DOP M-2043 M-2044 M-2043 M-2046 M-2047 Ale. Hark XI G-60
11. 12. 13 14.
15. 16.
10ft 0 II It ' . If II II
4tl 7 rt
it 11 11
11
il ls.
19. 20. 21. 22.
II II II II II II
11 it ii 11
11 11
2324. 25. 26.
II II It
11
ii
M
3
2'
The charts which follow contain the results of both heat and light tests run on the foregoing formulations (henceforth identified by formulation number). IVie Indicative numbers in each chart refer to the visual color and appearance of the exposure samples at the corresponding time.
Color Key Code:
0 Colorless : 1 Discolored
2 Lt. Yellow 3 Yellow 4 Lt. Amber
Amber Dark Amber Brown Black Spotted sample
Min. at 170C.
Heat Stability - Series "A"
8
10 11 12
14 12 lo 17 18 19
> I
I
I'M
DSW 620898 STLCOPCB4094926
f- * l: 4 I -r# 1-4#* -
V k f ** * ? f
Light Stability - Series "A" |
f. i r ' i-i ? I i f ' I
Hours 1 . 2 3 4 | 5 i 6
9 ; io; 1H 12! 13 14 15, l6t 17 18 12.
6
Heat Stability - Series
Min.
--" -----tr " 1
at I
170 il _2_i--h i
6
7
0 :9
10
11
12 Ul 14
15
16
17
18119 ----- 1--
.
0 5 0 1|111 1 :0 0 0 0 ` 0
20 40
p 6
3c2 \1 r>
6 ]6 05
6'; 0 iO
c2 4 "5
4 c,
4 2
OO 6 0 D 6 6 -- h 3 8
So O 6 6 8 3 l
0 1
2 6 8
1
3
6
0 1
5 6
01 Q__^
25 O
c rN
5 5 6
1 O
4 5 5
0
3 3 5
0 2
3 4 6
100 7 6
!
8668
120
111864000
! '
6
J
|
6
200 1
O
(Mj
-- '----1
-1-
21 22 23< 24 25 26
1
1 10
1-L 2
0 JT. O
0 c. 2
00 1 l1 2
01 1j
!
2 2 2 2 2 2i O4_ 2 3 2 2 2
3 23333
334 644
6 8 64 3 8 85 4
050
6 c;
86
Hrs. a |2
0 :4 ! 50 16 ; 100 i6 : 200 |7 ! 3Q0 '
4
Light Stability - Series "B" 5; 6 7 18 9 10 11 12 15 114 15 16 17 -1--8-->--1--9- 20 21 22 23 24 25 20;
8
5
s% 8
DSW 620899
STLCOPCB4094927
4p * e
kmp
* '* f I
i2. i: k * f i i
D. HB-40 Substitutes
In the light of an increasingly short supply of HB-40 for market consumption, various materials have been developed and examined as possible substitutes for HB-40 in vinyls. In the search for a satisfactory replacement, some exploratory products have been observed to be of interest because of performance and/or price. Others, however, were seen to possess few qualities of a usable nature.
The first consideration here will be the preliminary screening of the various potential substitutes which were submitted.
From these evaluations, the product ultimately considered as the most probable HB-40 substitute was chosen. The next part of this report contains a summary of the intensive evaluation results on that product, HB-20 (T-2, slightly hydrogenated). Two special reports have been previously written concerning this product, Special Application Reports No. 779 and No. 1005, both entitled, "Evaluation of HB-20 a3 a Substitute for HB-40", Job Nos. 117-2595 and II7-2616 (2), respectively, by P. R. Graham.
1. Exploratory Substitute Plasticizers for HB-40
The detailed results of the preliminary screening of all the exploratory products have been listed on Charts Nos. 1 and 2. They have all been studied as extender plasticizers, at various concentrations with DOP.
1,2 & 3 -- T-2, slightly hydrogenated (T-2 Is ethyl benzene still bottoms), T-2, moderately hydrogenated, and T-2-HB, slightly hydrogenated displayed fairly attractive compatibility as secondary plasticizers. Volatility of these, while high, is yet within the HB-40 volatility range. Other screening properties were well-balanced. These compounds appeared to be the most likely as HB-40 replacements. A more thorough consideration of T-2, slightly hydrogenated, may be found under part "E" of this same section of the report.
4 -- Chlorinated DDB (dodecyl benzene) high-boiler
wa3 one of four treated-DDB-hlgh-boiler samples submitted. The
other three, being slightly hydrogenated, half-hydrogenated, and
completely hydrogenated, respectively, were found to have no
practical compatibility, displaying no improvement over previous
DDB-hlgh-boilers, 'and were not subjected to preliminary screening.
The chlorinated DDB possessed an attractive balance of prooerties
at 1:3 DOP.
.
ii ;(j
gel
DSW 620900 STLCOPCB4094928
v 2 when incorporatedalone/| Jfoti
shore],hardness,; howeverjkl^pye
role Of primary* plasticizer.^!
HB-40.
'V1'".? S.*$
-I857) proved toJbeTcompatlble'
jIts -low^temperatui!i3^Leji$-:andl
ts, extreme 'inefficiencS|i|th(B f
:X:2.D0P, it was comparable' to ,
ir t
-
9,10, & 11 --;Epoxidized:lImonene dimer, (M-2073), ,
limonyl biphenyl (M-2074), and rosin oil (M-2075) all possessed equal plasticizing compatibilities, and while showing no more promise than any of the previous samples, they remained well within the HB-40 range of performance.
12 -- C22 aromatic tar, slightly hydrogenated (M-2076) was incompatible even when combined 1 pt.:3 pts. DOP. .
14 -- Indonex 632-1/2 (Indoil Co.), hydrogenated (M-2175) also possessed no practical compatibility.
13,13* & 16 -- Three other samples were found to have acceptable compatibility limits, and possess plasticizing proper ties within the performance range of HB-40. They were; heavy
aromatics (Eastern States Pet. Co.), hydrogenated (M-2174), T-2 (Texas City Stream 2) hydrogenated and H2S0* extracted (M-2176), and special anthracene oil XReilly) hydrogenated (M-2177).
2. Comprehensive Evaluation of HB-20 as an HB-40 Substitute
HB-20 is a slightly hydrogenated still residue from Texas City, a by-product formerly used only for solvent purposes. In a consideration of economics therefore, the potentiality of . HB-20 as^n^extender jplasticizer,^Qf* the HB-40 type, w&aivjryi i attractive". % In "view of this desirable quality, extensive testing of this material was felt to be warranted.
f
r In the course of the comprehensive evaluation of HB-20
vs. HB-40. two Special Reports were written, No3..779 and 1005, both
entitled Evaluation of HB-20 as a Substitute for HB-40", Job Nos.
117-2595 and 117-2616 (2), respectively, by P. R. Graham. In these
reports can be found all the detailed information that was obtained
and in addition, descriptive graphs and charts are presented there
in. Because of the completeness of coverage in those reports, only
a condensed summary,of that work, will be Included here." | | i :
. .# ; j Mr!
iKIlfeied favorablyin f '
most {tests
After a more intensive investigation^however,)
several shortcomings were, notec' *
- > , - **
DSW 620901 STLCOPCB4094929
i.
. 2. HB-20 suTfers a serious drawback in that it is unstable to light. No suitable ultra-violet light stabilizer has been found to alleviate the rapid yellowing that is character stic of HB-20 films after exposure to ultra-violet.
3. HB-20 is inferior to HB-40 and other commercial extender plasticizers of this type, in a consideration of vola tility and silica migration tests.
4. The relative volatility of this compound is believed to be the causative element in the heavy fuming and disagreeable, discomforting odor that is apparent during processing operations.
Since the completion of this work, K3-20 has been put on the market as a HB-40 replacement and Just recent!, has been considered for application in polyvinyl acetate adhesi/es.
VII. APPENDIX
Notebook pages used for this work:
A-33748, A-34497,.A-34498
A-389IO, A-389H, A-38921, A-38925, A-38926, A-38927, A-38928, A-38931, A-38932, A-38933, A-38934, A-38935, A-38940, A-38945, A-38946, A-38948
A-42701, A-42702, A-42703, A-42704, A-42705, A-42706, A-42707, A-42713, A-42714, A-42715, A-42718, A-42719, A-42726, A-42727, A-42740, A-42750
A-44458, A-44469
A-44663, A-44664, A-44665, A-44687, A-50964
I: \ $ nd
L. R. Wangler J. H> Darbyj
DSW 620902 STLCOPCB4094930
* - * #mmm ** *
STLCOPCB4094931
9mmm. mm&m# imamm* *
STLCOPCB4094932