Document pxjEyd9eYy93qk77jEaq1K0E

zr> & o '4 o. "g BUSINESS se CONFIDENTIAL Q"2 " <. -i ai IS- -5g uJ <<! $< CD u d > I 5 ^ Preliminary Information Subject to Later Verification or Revision "DOO e | JS 5 $ 8 41J INFORMAL REPORT < tr> >. > grgj^rfct'Jo. J452--M33 File No. Date 3, 1969 Author (s) Ingalls j*--- - - '*"---3 iPlASTlCS INVESTIGATION OP THE COWLES DISSOLVER Fflft DI5PER5I&M OF RE5IM-0RAPE ASBESTOS BkObUcTs In epoxy and polyester resins SUMMARY The Cowles Dissolver, which is comparable to mixing equip ment used in the plastics industry, has been found effective for dispersing both R-G244 in polyesters and R-G144 in epoxies. The intrinsic viscosity of the base resin and level of asbestos added are the principal factors determining the amount of energy and mixing time required for optimum dispersion. In the range of R-G244 additions normally recommended for thixo tropic polyester resins, operating conditions approximating 3000 rpm (^'2400 PPM peripheral tip speed) for 10 to 20 minutes are adequate for proper dispersion with a Cowles Dissolver. Good dispersion of R-G144 In epoxy systems requires approxi mately 3400 rpm (>-'2700 PPM peripheral tip speed) for a period of 20-40 minutes with the Cowles Dissolver. The operating conditions recommended above should apply for most resin-grade applications where viscosity of the thixotropic system is below 30,000 cps equivalent at 6 rpm Brookfield viscosity. EXPERIMENTAL A Cowles laboratory dissolver was used for this investiga tion employing a 3" impeller. The mixing speeds were at 2000 and 3400 rpm, respectively. These data were compared to a laboratory Homo-Mixer, 4 blades, 2" diameter atrr.5000 rpm. Mixing time was varied between 3 to 40 minutes. Rohm-Haas Corporation Paraplex P-43 was used for the poly ester resin and diluted with styrene to a base viscosity of 100 cps. The epoxy used was UCC ERL-2796 having a base viscosity of 150 cps. Research and Development Department Chemicals and Plastics Union Carbide Corporation Niagara Falls, New York A 1723 1 BUSINESS CONFIDENTIAL Viscosity measurements were obtained with a Brookfield viscometer at 25C, All samples were hand stirred prior to measure ment for viscosity. DISCUSSION 1. Mixing Requirements for R-G244 in Polyester Applications The mixing parameters required for optimum dispersion of R-G244 in polyester resin with a Cowles Dissolver are illustrated in Table I and Figures 1 and 2. Results show Cowles equipment to be effective for dispersing R-G244 in polyester resins. However, a minimum of 2000 rpm was required for 40 minutes to obtain an optimum viscosity at a loading of 0,5 phr R-G244. Approximately 10 minutes were adequate for R-G244 dispersion at 3400 rpm. It is apparent that the intrinsic viscosity of the base resin and level of asbestos added are the principal factors determining the amount of energy and mixing time required for optimum dispersion. At the higher levels of R-G244, 1,0 to 2.0 phr, a minimum of 20 minutes mixing was required at a setting of 2000 rpm to disperse the R-G244, Samples prepared in less time contained visible lumps of asbestos. Additional mixing beyond 2u minutes decreased the viscosity, apparently due to degradation of the R-G244, Mixing 1,02e 0 phr R-G244 at 3400 rpm was indicative of optimum viscosities between 5 to 10 minutes. At the 0,5 phr level of R-G244 normally recommended for thixotropic polyester laminating resins, operating conditions approxi mating 3000 rpm (52400 FPM peripheral tip speed) for 10 to 20 minutes should be adequate for proper dispersion with a Cowles Dissolver, 2, Mixing Requirements for R-G144 in Epoxy Applications The efficiency of the Cowles Dissolver for incorporating R-G144 in epoxy resins is shown in Table II and Figures 3 and 4. Longer mixing time was required to disperse R-G144 in epoxy resin than was observed with R-G244 in the polyester system. A level of 2000 rpm on the Cowles Dissolver was not enough shear for adequate dispersion within the practical limits of mixing time. Based on these data, mixing conditions required for good dispersion of R-G144 (less than 2 phr) in epoxy resins should approximate- 3400 rpm (^p.2700 FPM peripheral tip speed) for 20-40 minutes with the Cowles Dissolver, -2- A 17232 BUSINESS CONFIDENTIAL Again it should be emphasized that optimum mixing condi tions will vary depending upon the base viscosity of the resin system, The rate of energy input to the system is a direct function of viscositye However, conditions recommended herein should apply for most Resin-Grade Asbestos applications where viscosity of the thixotropic system is below 30,000 cps at 6 rpm on a Brookfield viscometer. BLI/bsn Attach, Distribution: Messrs, R, E, Byrne W, L, Carrick G, Lo Dickson J, L. Myers H. Bo Rhodes y J. A, Riddle'S No Jo Setter J, E, Skvarla Wo So Young File - 10 B.VL, Ingalls -3- &17233 BUSINESS CONFIDENTIAL TABLE I EFFECT OF SHEAR FORCES ON THE RHEOLOGICAL PROPERTIES OF R-G244 ASBESTOS IN POLYESTER re^Tn* R-G244 (phr) 0.5 0.5 0.5 0.5 1.0 1.0 1.0 2,0 2.0 2.0 2.0 Mixing Time (Min.) 3 5 20 40 5 20 40 3 5 20 40 Brookfield Viscosity (cps) at 25C and 6 : Cowles Cowles Homo-Mixer 2000 rpm 3400 rpm 2^5000 rpm 850 675 725 775 725 - 850 700 - -- - 25,500 24,000 20,000 5000 4600 4400 25,500 22,000 13,500 -- - 19,500 - mm - Polyester Resin - Rohm & Haas Corp, Paraplex P-43 polyester (base viscosity adjusted to 100 cps with styrene) Mixing Parameters: Cowles Dissolver - 3" diameter impeller Homo-Mixer - 4 blades 2" diameter j\ 1 7 23 A- BUSINESS CONFIDENTIAL TABLE II EFFECT OF SHEAR FORCES ON THE RHEOLOGICAL "------R-U14i 'A'SB'ESTflS'IN------------------------------------------ ETOXY BESIH*--------------- R-G144 (phr) 1.0 1.0 1.0 1.0 2.0 2.0 2.0 2.0 Mixing Time (Min,.) 3 5 20 40 3 5 20 40 Brookfield Viscosity (cps) at 25C and 6 2000 rpm 00 rpm ^5000 rpm 625 1100 1450 . 1800 2700 2800 2900 _ _ - 3400 6500 8600 10,500 10,000 10,000 13,000 -- - *Epoxy Resin - Union Carbide Corp, ERL 2796 epoxy (base viscosity 150 cps) Mixing Parameters Cowles Dissolver - 3" diameter impeller Homo-Mixer - 4 blades 2" diameter 17 23b