Document pmkYd1ad3wjZGbqb7q5ORnyNd
Reference 1
An economic, commercial process for
Detoxifying PCB-Contaminated Transformer and Heat-Transfer Fluids
By D. K. PARKER and W. L. COX, Th Goodyear Tire and Rubber Co , Akron. OH
SAIF disposal of highly toxic polychlorinated biphenyl (PCB)
ises, preferably in existing equip ment
transformer and heat-transfer flu a Handle either small or large vol
ids long a perplexing problem for umes of materials
plant engineers (see section "The Have relatively low equipment
Major steps in the process arc shown in Fig. I. The method used to
convert the PCB-contaminatcd flu ids consists essentially of causing the fluids to react with an organo-
FCB Disposul Dilemma")--is now feasible, using u recently developed
and operating costs.
sodium reagent, sodium naphtha-
chemical treatment process. The treatment, which is also applicable
REAGENT PREPARATION STEPS
to other halogenated contaminants
such as polybrominalcd biphenyls
and DDT tctrachlurobenrodioxin
pesticides and herbicides, extracts
the toxic ingredients and converts
them into a nontoxic residue that
can be safely incinerated in conven
tional equipment. The contami
nant-free fluids can be recovered
for reuse.
1 he process has been successfully
used on a large scale at a Goodyear
plant. Hatches of PCB-contami-
Ruled heat-transfer fluids, ranging
in si/c from 100 to 2000 gal. have
been converted to environmentally
acceptable substances. Typically.
PCI) content has been reduced from
82 ppm to less thun 10 ppm--well
PiQ. 1. Batch process converts PCB contamlnatad haat-transfar fluids into
below the Fnvironmentnl Protec tion Agency's (I PA) 50 ppm max
nontoxic rtsidut capabls of being safely indnaratad by conventional equip ment. Contaminant-free fluids art recovered for reuse.
imum permissible limit. The F.PA is
evaluating the pnxe.ss and patents
are pending. When grunted, the
patents will be dedicated to the
public and the process will be made
avuiliible for widespread use. Target Goals--The following
gouls were established when the technique was developed. The pro cess should o Permit pomplcte. yet selective,
Pig 2. A minimum S0-to-100 gram motocuiar weight ratio of sodium naphthalido to cNorino la noodad to
romovo 96 parent of PCB from standard hoal-tranafar fluid containInQ 62 ppm of PCB.
conversion of chlorinated sub
stances to nontoxic, easily dispos able products lie capable of use on plant prem
- SODIUM NAPHTHALIOt- TO
CHLORINE PROPORTIONS, MOLECULAR WEIGHT RATIO
ru 7M0
AUGUST 31. I960 PLANT ENOitJEtniNG 133
HONS 0 0 9 2 5 2
"Tha r--ctlon daatroya tha chamlcal bond* that pravfoualy hatd tha PCBa togathar and craatad tha toxic affacta. "
Tho PC0 Disposal Dilemma
Tfta kfsal fluid for electrical equipment end heal-tranafer systems has excel lent t>eet stability, a non-flammable nature, low votatiiity, and good viscosity Cheracteristics at operating temperatures These properties are charactr sties Of some chlorinated aromatic compounds that have found widespread use as a family of related malarial* known as Aroctors and aekareta
Howaver, subsequent events heve demonstrated that coupled with their desirable properties, these materials (collectively known as polychlorinated
biphenyls or PCBs) also heve undesirable properties that can causa health problems The Chemical stability and environmental persistence of PCBs. cou pled with their widespread use in the 1960s end 1970s. indicated the possibility of potential health hazard to tha public
Their manufacture was discontinued and EPA regulations were issued under ttie authority of tha Toxic Substances Control Act to control the materials currently in use In the O S The regulations became effective July t, I960. They
dohne any materiel containing 60 ppm or more of a mono- or polychlorinated biphenyl as a PCS and regulate its use and disposition. Currently, tha only
permissible dispout of a PCS is by incineration in an SPA-approved incinerator (nonu axial) or by burial in an EPA-approved landfill.
Either method requires transportation from the point of use to tha disposal site, thereby Increasing tha chances of inadvertent release into the environ ment Furthermore, the siting of Incinerators to burn PCBs has met strong opposition from local residents of areas under consideration. Consequently, the chemical conversion of PCBs to environmentally acceptable by products Is a most desirable solution.
MATERIAL COSTS FOR TREATING HEAT-TRANSFER FLUID CONTAINING 62 PPM OF PCBs
Materiel
Amount required to treat 100 lb of oil, lb
Coet/tb, Cot/100 lb dollars* of oil, dollars
Sodium
0,1098
060
Healttensfer oil
(PCB contaminated) Nufihthelene
1.0994 0 7029
---- 0.36
Tetiahydiofuran
Tom
1.9525
' 0 86
`Puces Hand in ChtmcatMtr*Ming OtpOflm. February Yd. I960. Unit cost depends on quantities purchased.
00747
0.2530 1.6792 2.0069
lidc. The reaction destroys the chemical bonds that previously held th.- PCbrf together and created the toxic effects.
The reaction takes less than 5 min under an inert atmosphere (ni trogen) it room temperature in glass or itcel vessels. A minimum mole ratio of sodium nuphthalide to chlorine of $0 to 100 is required to remove 98 percent of PCBs from a standard heat-transfer fluid con taining H2 ppm of PCBs, Fig. 2.
Only small amounts of heat are generated when the reagent is mixed with the heat-transfer fluid and when the reaction is taking place. Although the reaction is es
sentially completed in a matter of
minutes, the mixture is held in the reactor for several hours to ensure complete reaction Following this holding time, the solution is quenched with water and distilled under vacuum to recover the re agent and the contaminant-free heat-transfer fluid. The residue re maining after distillation consists of
non-halogenated potyphenyls and sodium chloride that can be safely incinerated.
Reagent Preparation--The pro cedure for preparing the reagent is relatively simple but requires care ful control. Approximately ISO to 400 mL of either fresh or contami nated heat-transfer fluid per gramatom of metallic sodium pieces arc
134 FIAMT CNCHNEEMNO O AUOUST 21. 1660
charged to the reagent preparation vessel. The mixture is then vigor ously stirred at 300 to 340 F for 5 to 10 minutes under an inert (nitro gen) atmosphere.
The treatment produces highly reactive, finely dispersed, liquidsodium droplets. Agitation is con tinued uTiilc the mixture is rapidly cooled to room temperature. Cool ing causes the sodium droplets to solidify into line, bright spheres
A (ctrahydrofuran solution of naphthalene is then added to the mixture The addition instantly be gins to produce the organo-sodium reagent, sodium naphihalide. as ev idenced by the formation of a char acteristic greenish-black color. Gentle, additional stirring for 1 to 4 hours completes the preparation of the reagent, which is then ready fur use. At this point, the reagent solu tion is homogeneous.
However, it is imperative iliut extreme caution be taken with all reactions involving metallic sodium. Rapid generation of hydrogen oc curs when sodium makes contact with water. For this reason, care must be taken to ensure that no metallic sodium enters the PCBconvtrsion-rcaetion vessel. Also, during the water quench step, the water must be added in small amounts over a long period to mini mize possible hydrogen release Ni trogen or a similar inert gas is used as a blanket to prevent the form ition of potentially explosive hydro gen/oxygen mixtures.
Economics--Chemical material costs for the PCB treatment process arc about $0.02 per pound of recov ered hcal-transfcr fluid, compared to SI per- lb for newly purchased fluid. The cost docs not include sav ings realized from naphthalene and tetrahydrofuran recovery, which can be significant in large-scale op erations. Data for large scale treat ment of lient-transfcr fluid contam inated with 82 ppm of PCBs are shown in the accompanying table.