Document pmgRjBn7mYjmoO0xRdDq601ej
rtT\|Tl
VU'ID
APPLICATION DATA BULLETIN No. P-115
Manufactured by
Monsanto Chemical Company '
ST. LOUIS, U. S. A.
Boston Birmingham Charlotte Chicago Cincinnati Cleveland Detroit Lob Angeles New York Philadelphia San Francisco Seattle * Montreal London 0222000
TOWOLDMON0026621 WATER_PCB-00011090
FOREWORD
The Aroclors*, chlorinated biphenyl and chlorinated poly-phenyls, possess unique properties which enable the fulfillment of requirements not met by other materials. This has won a prominent place for Aroclors, particularly, in the electrical insulating: field and in such widely differing applications as non-flammable hydraulic media, hightemperature and high-pressure lubricants, heat transfer and expansion media, sealing compounds, adhesives and protective coatings, including plastics, pigments, lacquers, paints and varnishes. This booklet describes the properties of thirteen Aroclors, each of which is representative of a series. For almost every Aroclor described there is a dark-colored grade of other wise approximately the same physical and chemical char acteristics. These darker products arc less pure but lower in price. The Aroclors are efficient and very economical, both when used alone to accomplish results not attainable by other materials and when used as extenders to enhance the properties of other products. They are produced exclusively by Monsanto Chemical Company.
^Registered in V. S. Patent Office.
022*001
TOWOLDMON0026622 WATER_PCB-00011091
INDEX
Page No.
GENERAL PROPERTIES..................................3
General Physical Properties of Some of the Aroclors.............................................. 4--5
Resistance of Structural Materials to Aroclors ...................................................... 6
Adhesiveness....................................................... 7 Coefficient of Expansion.................................. 7 Corrosion...............................................................7 Density................................................................... 7 Electrical Properties..........................................9 Non-drying Properties...................................... 9 Nonflammability.................................................. 9 Solubility...............................................................9 Specific Heat and Thermal Conductivity . 9 Thermal Conductivity of Aroclor 1248 . . 9 Stability............................................................. 10
Toward Alkalies............................................ 10 Toward Acids................................................ 10 Toward Heat.................................................10 Toward Oxidation........................................ 10 Surface Tension................................................ 10 Thcrmoplasticity.................................................10 Toxicity............................................................. 13 Vaporization Loss.............................................13
APPLICATION OP AROCLORS....................14 Adhesives............................................................. 14 Electrical^Equipment........................................ 14
Page No. Expansion Medium............................................ 14
Hydraulic Medium............................................ 14 Power Transmission....................................14 Hydraulic Pressure Medium........................14 Gaskets ............................................... 15 Liquid Heating Medium............................15
*
Lubrication........................................................ 15 Air Compressors............................................15 High Temperature........................................ 15 Extreme Pressure........................................ 16 Submerged Lubrication................................ 16
Suggested Uses for Aroclors in Plastics, Pig ments, Lacquers, Paints and Varnishes 17
Compatibility with Various Materials . . 17 Ethyl Cellulose . .........................................17 Graphic Arts.................................................17 Impregnation.................................................18 Moisture Proofing........................................ 18 Nitrocellulose Coatings................................ 18 Pigment.........................................................19 Paints and Varnishes.................................... 19 Rubber and Rubber Substitutes .... 19 Modified Rubber Finishes........................... 24 Vinyl Resins.................................................... 24
Diagrams Showing Practical Composi tion of Lacquers Using Aroclors 1254 and 1262 ......................................... 21-22-23
2 02*Z02
!
TOWOLDMON0026623 WATER_PCB-00011092
General Properties
The Aroclors range in form and appearance and Aroclor 5460 is insoluble in the lower
from mobile oily liquids to fine white crys molecular weight alcohols. Aroclor 4465 is
tals and hard transparent resins. They are only partly soluble in the lower alcohols.
non-oxidizing, permanently thermoplastic, of low volatility and non-corrosive to metals. They are not hydrolyzed by water, alkalies or acids. The viscous liquids and the resins will not support combustion when heated alone.
The excellent electrical properties, fire resistance and inertness of the Aroclors make them useful in many applications.
The properties imparted by the Aroclors and their usefulness for particular applica
The crystalline Aroclors are relatively insol tions vary in regular gradients over the
uble, but the liquid and resinous products series so that the selection of the right
are soluble in most of the*common organic Aroclor for a specific use can generally be
solvents, thinner* and oils. All Aroclors are made simply by a comparison of the physi
insoluble in water, glycerine or the glycols, cal properties of the several Aroclors.
3 022203
TOWOLDMON0026624 WATER_PCB-00011093
TABLE
GENERAL PHYSICAL PROPERTIES
Form....................................................................... Color--APH A............................... ......................
Aroclor 1221 Colorless mobile oil (
50 Max.
Aroclor 1232 Aroclor 1242 Arcolor 1248
Practically
Practically
Yellow tinted
colorless mobile colorless mobile mobile oil
oil oil
60 Max.
100 Max.
100 Max.
Aroclor 1254 Light yellow viscous oil
150 Max.
Acidity--Maximum (Mgm. KOH per Cm.)- 0.015
0.015
0.015
0.015
0.015
Coefficient of Expansion.............. cc/cc/*C
Density-- Specific Gravity 25"/'25"C (77777F).......... Pounds per Gallon--25C (77F)..................
0.000707 (15-40*C)
1.177 to 1.187 9.82
0.000725 (25"-100"C)
1.262 to 1.272 10.51
0.000678 (25"-65"C)
1.378 to 1.388 11.50
0.000702 (2S"-65"C)
1.447 to 1.457 12.08
0.000661 (25-65C)
1.538 to 1.548 12.83
Distillation Hance--ASTM D-20................ Mod Corr. C................................................... 275*-320
Evaporation Loss--%--ASTM D-6 Mod. 163*C........................................................ 5 lire. -- 100"C........................................................ 6 hra. 1.0 to 1.5
290-325*
-- 1.0 to 1.5
325-360
3.0 to 3.6 0.0 to 0.4
340*-375*
3.0 to 4.0 0.0 to 0.3
365*-390
1.1 to 1.3 0.0 to 0.2
Flash Point--Cleveland Open Cup............*C 141M50 "F 286*-302
Fire Point--Cleveland Open Cup.............. C 176 F 349*
Pour Point--ASTM D-97........................... C "F
Softening Point--ASTM E*28.................. *C
Crystals at l*C Crystals at 34%
--
"F --
Refractive Index--D-linc--20C.................. 1.617-1.618
Viscosity--Saybolt Universal 210F (98.9*C) 30-31
See. (ASTM--D-88)
13rF(5,4T,, 35-37
100T (37.8C) 40 42
152"-154" 305"-310"
238* 460
-35.5"
-32
-- -- 1.620-1.622
31-32 39-41 47-50
176"-180" 348"-356"
334* 633*
-19*
2*
-- --
1.627-1.629
34-35 49-56 80-93
193"-196 379"-384" None
7* 19.4"
-- 1.630-1.631 36-37 69-78 185-240
None
None
10* 50* " 1.637-1.641 44-18 260-340 1800-2500
TOWOLDMON0026625 WATER_PCB-00011094
/
OF SOME OF TIKE AIIOCLORS
Aroclor 1260 Light yrJlow soft sticky resin ISO Max.
Aroclor 1262 Light yellow sticky clear resin 150 Max.
0.015
0.02
- 0.000640 (25-65C)
1.618 to 1.629 1.646 to 1.653
13.50
13.72
Aroclor 1268
Pale yellow opaque brittle resin 1.5 Max.
Aroclor 1270 Aroclor 4465
White ervs- Yellow trans*
taliinc powder parent brittle
resin
1.5 Max.
2.0 Max.
Aroclor 5442 Yellow trans* parent sticky resin 1.5 Max.
Aroclor 5460 Yellow trans* parent resin
2.0 Max.
Aroclor 256' Brown*black opaque resin
~
0.05
0.175
0.05
0.05
0.07
1.4
-
0.000611
0.00123
0.00179
(25-65C)
(25-99C)
(25-124C)
1.804 to 1.811 1.914 to 1.960 1.712 to 1.723 1.432 to 1.147 1.740 to 1.745
15.13
16.24
14.28
11.96
14.50
0.000656 (25-65C)
1.724 to 1.740 14.41
385"-420"
0.5 to 0.8 0.0 to 0.1
None
None
SI* 88 -- 1.647-1.619 75-80 3200-4500
400"^!30"
0.5 to 0.6 0.0 to 0.1
None
None
37 99" -- 1.6501-1.6517 00-103 600-850 (I60*F or 71C)
435-450"
0.1 to 0.2 0.0 to 0.06
450"-460
0.0 to 0.1 0.0 to 0.02
230-320
215*-300*
280-335
at 4 mm. lig. at 4 mm. Hg. at 5 mm. Hg.
0.2 to 0.3 0.0 to 0.02
2.0 0.05
0.03 1.5 to 1.7 (at #60*--5 kr.
-
0.2 to 0.3 -
None
None
-- 135 to 160 (hold pt.) 275 to 320 (hold pt.) --
--
None
None
249 to 300 (hold pt.) 561 to 572 (bold pt.) -- -
None
None
60 to 66 140 to 151* 1.664-1.667 90-150 (SWF or 1)0*C) --
247 477
None
>350" >662"
None
46 115" 45 to 50 113' to 122".
100 to 105.5 212" to 222"
-- 300-400
1.660-1.665
--
None
None
1
-
66* to 72
1
149 to 162 I
--I -I
--1
0222005
TOWOLDMON0026626 WATER_PCB-00011095
TABLE 1J-- Resistance of Structural Materials to Aroclors
Metals
12.48
25BC
125C
Aroclor Ni/mbf.r
1254
25C
125BC
4465 125BC
5460 125*C
Aluminum...................................................................... Copper............................................................................ Magnesium.................................................................... Nickel.............................................................................. Silver............................................................................... Tin................................................................................... Zinc.................................................................................. Mild Steel....................................................................... Phosphor Bronze.......................................................... Red Brass..................................................................... Stainless Steel............................................................... Yellow Brass..................................................................
R R RR RR R R R RR R D RR R
R D R R R R R R D D RR Re
RR DR RR R RR RR RR RR RR RR RR RD RR RR R De
*RR D RR RR R R R R R R RR Re
RR D RR R R R RR HR R De
RR Re
Plastics
Alkyd Resin No. 4659-1-12......................................... P
P
P P
P
P
D P
D P
P
P
Butvar Low Plasticized.............................................. D
T
DT
T
T
Butvar Themoset......................................................... P
P
P P
P
P
Cellulose Acetate (Fibcstos)...................................... D
P
DP
P
P
Cellulose Nitrate (Nitron 205D).............................. D
T
DT
T
T
Durite Phenol Furfural Resin................................... D
P
*R P
DP
Ethyl Cellulose (Ethofoil).......................................... *R
P
D P
P
P
Formvor Highly Plasticized....................................... De
T
Pe T
T
T
Forinvar Low PlaBticizcd........................................... PS
T
PS T T T
Glyptal 1276.................................................................. R
P
DP
P
P
Glyptal 7136.................................................................. D
T . R
T
T
T
Maleic Resin No. 46394-13B..................................... P
P
P P
P
P
Maleic Renin No. 46394-13C..................................... P
P
R P
P
P
Plexiglas (Methyl Melhacrvlate)............................. D
P
*D P
P
P
Polystyrene (Liislron B)............................................ P
T
PT
T
T
Resinox Mineral Filled Melamine Resin................ D
P
R R
P
D
Resinox Mood Flour Filled Melamine Resin........ D
P
R D
K
P
Resinox Mineral Filled Phenol Formaldehyde.... *D
D
*D D
R
P
Resinox M ood Flour Filled Phenol Formaldehyde D
P
D R
D
P
Resinox ltag Filled Phenol Formaldehyde............. D
D
*D D
D
P
Urea Formaldehyde Resin (1`luskou Co.)............... D
P
D P
P
P
Vinyl Acetate (Gelva 60). ........................................ D
T
PT
T
T
Yinyl Chloride (Vinylite)........................................... RR
T
RR T
TT
Meaning of Abbreviations: *--Based on weight gain calculated as |enetration value shown.
RR--Excellent resistance--less than 1.0 x 10 ' cm/day penetration or .00014 in/y r. R--Good resistance--lias iienetrathm between 1.0 x 10' and 10 x 'I0'cm/day or between 0.00014 and 0.0014 in/yr. D--Doubtful resistance, penetration between 10 x 10' cm/day and 100x10' * cm/day or between 0.0014 and 0.011 in/yr. P--Poor resistance--penetration greater than 100 x 10` cm/day or 0.14 in/yr.
PS--Poor resistance due lo visible local action although weight change indicates greater resistance, e--Following the letter indicating resistance signifies material niuv be better than indicated if totally immersed - since weight loss is believed to come from oxidution of the part of test strip exposed to air. T--Material alone wilt not stand tem{erature.
#
021100b
}
TOWOLDMON0026627 WATER_PCB-00011096
Adhesiveness
The Aroclor resin* ahderc strongly to smooth surfaces. nucli as glass, metal ami varnished or lacquered coatings. The softer Aroclors are indicated when* a flexible, Iton-drviitg. water-resistant strongly adhesive ma terial is required. The Aroelor adhesives are thermoplastic; are readily applied hot without solvent: do not require high temperatures for easy application, and are set immediatclv upon cooling.
Coefficient of Expansion
Specific Volume
Temp. F 0
100 200 300 400 500 600
Aroclor 1248 S|*ecific Volume ml gm
0.674 0.699 0.726 0.755 0.790 0.828 0.870
Using the simple formula Vt *= Vti [1+a (t --ti)]* the coefficient, , has been calculated at 100F increments, as follows:
Temp. Range "F
0 to 100 100 to 200 200 to 300 300 to 400 400 to 500 500 to 600
Coefficient of Expansion
0.000371 0.000386 0.000399 0.000163 0.000481 0.000507
Corrosion
The Aroclors show practically no corrosive effect on metals within normal ranges of temperature. They do attack manv plastics materials of con struction as shown in Table 11.
Density
All the Aroclors are heavier than water, a valuable property for many applications. Densities are shown in Figure 1.
ISO
A b s o l u t e D e u s it t ( g m s . / cc)
/ 70
Dai13/r/E.5 04/4/?oct 0/23 AT VAx/O 'JS 72.MPC&47-0X23
1.60
ISO
1.40 %
ISO
1.20
/.to 40 30 120 !S>0 200 240. 260 320 360 400 440 T214P/?Aru2C 0202225 C
7
0222007
TOWOLDMON0026628 WATER_PCB-00011097
DIELECTRIC CONSTANT <> 1000 CYCLES
FIG. 2
O fsj
n
rov o
I
TOWOLDMON0026629 WATER_PCB-00011098
Electrical Properties
The Aroclors have extremely interesting electri cal characteristics: high resistivity and dielectric Strength and low power factor. The dielectric con stant ranges from 3.4 to 5.0 at KKPC and 2000 cycles, depending upon the particular Aroclor.
The dielectric constants of Aroclors 1212 and 1254 at various temperatures are shown graphically in Figure 2.
Non-Drying Properties
The Aroclors arc non-drying, and when they are exposed to the air, even in thin films, no notice able oxidation or hardening takes place. How ever, when used as ingredients of lacquers, they do not retard the rate of drying of the lacquer films. Quick drying varnishes and paints may be made with Aroclor resins.
Nonflammability
The viscous Aroclor oils and the resins do not support combustion when heated alone, even at their boiling points-- temperatures above 350C. Most of the Aroclors (tux readily with resinous and pitch-like materials to give a product hav ing a decreased fire hazard. When incorporated in nitrocellulose films and rubber foams the Aroclors retard the rate of burning.
Solubility
All Aroclors arc insoluble in water. Solubilities of some of the Aroclors in the more common sub stances are shown in Table VI.
The Aroclor oils and resins are readily soluble in most of the common organic solvents and drying oils. The hard crystalline materials are in general less soluble than the Aroclor oils or softer resins. Compatibility data on Aroclors in nitrocellulose lacquers are shown on page 18.
Specific Heat and
Thermal Conductivity
The specific heat at different temperatures of several of the Aroclors is shown in Figure 3. This, together with the thermal conductivity data given in Tabic IV, enable calculations involved in the use of Aroclors as higli-tcmpcrature, low pressure, fluid hcat-transfcr media.
TABLE IV
Thermal Conductivity of Aroclor 1248
Temperature
C F
30 90
60 140 100 212
Thermal Conductivity Viscosity
Density BTU./Hr./Sq. Ft./ Saybolt
g/cc.*F/Ft.
Uatv. Sec.
1.441
0.0613
360
1.411
0.0698
60
1.370
0.0800
36
TABLE III -- Electrical Properties
- Aroclor 1232
Dielectric. Constant @ 100C and 1000 Cycles...................... 4.6
Aroclor 1242
4.9
Aroclor 1248
4.6
Arocix>r 1254
4.1--4.3
Resistivity 100C Ohms/Cm* 500 Volu D.C.........................
500 x10
Above 500 x 10*
Dielectric Strength..................... Power Factor (100C, 1000 kc)
IKS Method 11-3953871. ASTM 1)177-11.
less than 0.1%
35 KV Min.
eo
T
Aroclor 1260
Above 500x10* 30 KV Min.
Aroclor 5442 4.9
1469 x 10*
less than 0.1%
O
0222009
|
TOWOLDMON0026630 WATER_PCB-00011099
FIG. 3
Even prolonged treatment (255 hours) with con centrated sulfuric acid indicated only a slight trace (too small for quantitative measurement) of hydrogen chloride in the acid layer.
Toward Heat
Because of their stability to heat, the Aroclors are useful heat-transfer media. Aroclor 1254 and particularly the less viscous Aroclor 1248 are recommended for this purpose because they may be heated at temperatures up to 315C (600F) in a closed system for long periods without appreciable decomposition and are at the same time nonflammable.
Toward Alkalies
The Aroclors are remarkably resistant to the action of either hydrolyzing agents or high tem perature. They are not affected by boiling with sodium hydroxide solution.
Toward Acids
Experiments were made to determine whether hydrogen chloride is evolved during the treat ment of Aroclors with sulfuric acid. Aroclor 1254 (selected as typical) was stirred with an equal vol ume of ten per cent sulfuric acid for a period of 150 hours. Auy gases escaping from the reaction flask had to pass through a trap filled with silver nitrate solution, whirh solution would give a pre cipitate of silver chloride if any HC! came in con tact with it. After 150 hours of treatment, neither the trap solution nor the acid layer in the treat ing flask showed anv hydrogen chloride present.
Toward Oxidation
When Aroclors are subjected to a bomb test at 140C with 250 pounds oxygen per square inch oxygen, there is no evidence of oxidation as judged by development of acidity or formation of sludge*
Surface Tension
The surface tension of Aroclor 1254 in dynes per centimeter is a6 follows:
Temperature 25C
80C 100C
Surface Tension--dynes ,/ce ' .... Soi
44.0 42.0
Thermoplaslicily
The Aroclors are permanently thermoplastic. They apparently undergo no condensation or harden ing upon repealed melting and cooling. The clear Aroclor resins arc now being produced with soft ening points up to 105C. The opaque crystalline solids arc produced with initial inciting points up to approximately 290C.
10 0Z2210
TOWOLDMON0026631 WATER_PCB-00011100
TABLE 17-- Solubility of Aroclors in 100 Milliliters of Various Solvents
Aroclor AcTtyfpPe of Solvent
25'C
1248 25flC ilot
1254
25C
Hot
1270 Cold Hot
Acetic Acid................................. S
Oleic Acid.................................... S Benzoic Acid............................ I0.CJI'c
--_
s s
s __ s -- --.
10.0 wc -- -- --
"
Aldehyde 40% Formaldehyde...............
I
I-
II
I
I 11
Furfural................................... VS
VS
vs vs vs vs SS SS
Atnioe
Aniline...................................... S Pyridine....................................132.5 M'c
S 440 wc
-- s s --_
--
--
114 s,*c 42$ io**c --
--
Chloro--derivative Amyl chlorides -- mixed.... S Carbon Tetrachloride........... S
Chloroform.................................. S Dichlorethylene......................... -- Ethylcue Dicliloridc.................. S Monochloroltcnrene.................. S Orthodiclilorobenzeue.......... "
Tetraclilorethane....................... S Trichlorelhane........................... S Triclilorcthylene........................ S
S S
s
s s
s s s
ss ss ss
ss ss
ss ss ss
s S __ --
s S 3.7 --
_s
S __ -- 3.0 --
T s ----
s s 2.9 --
_s
s s
s-- s 3.3 -- s ----
Drying Oil Tung Oil...................................... Linseed Oil..................................
S S
s s
s s s s __ _ s s s s ----
Ester Amyl Acetate............................. Butyl Acetate............................. Cetlosolve Acetate..................... Cottousced Oil........................... Dibutyl IMithalate................. Diethyl Phthalate................. Ethyl Acetate......................... Ethyl Lactate.........................
Ethylene Glycol Diacetatc.. Methyl Acetate..................... Tricresyl Phosphate..................
Ether: Ethyl Ether......................
S S S S S S S S
S S
S
S
s s s s s s s s s ss s
s s s s __ ' __
ss
s s
ss
s ----
s ----
Ether Alcohol Carbitol................................... 224 Cellosolve.................................... S
307s99,0
vs s
vs s
173 *`*c 259 9#,c -- s S ----
Diethylene Clycol................. -- P`P' Diliydroxy Ethyl Ether 16.9 :5c
19 *c
ss ss
8 `C 10 100*C -- --
llydcocarbon Benzene....................................... VS
Gaaoline...................................... VS Kerosene..................................... VS Mineral Spirits....................... VS Paraffin. ..............................2.0
Pine Oil........................................ S Toluene.................................... VS Turpentine.............................. VS Xylene...................................... VS
vs vs
vvss
ss vs vs vs
Hydroxy -- derivative
sAmyl Alcohol............................. S sn-Dutyl Alcohol......................... S
,0*cEthyl Alcohol (3-A).......................23.3***c80.0
Glycerine..................................... I
1
Methyl Alcohol...............................42.5*'c 88.5 tc'i:
sPhenol -- 90%................................. 194*`c
vs vs vs
2.0vs*c
vs vs vs vs
__ __1
__
--
vvss
vvss s vs vs vs vs
_ __ I
--
vs
vs
vs
vs
---
s
-
vs vs
vs
s s
10 I
15ss
VS vs vs vs s vss vs vs
s s
28 I
22.2
S
3.5 _
---- --
--
----
----__ --
----
--
--
_
----I
----
1
-- ---
Ketone Acetooe........................................
S
s
----
s
s ---
Miscellaneous
Carbon Disulfide....................... S
Nitrobenzene.............................. S
Water........................................... I
1 -- Insoluble
S -- Soluble
SS -- Slightly Soluble
VS -- Very Soluble
Figures show grains of Aroclor per 100 milliliters of solvent at 25C unless otherwise indicated.
446S Cold Hot
SS s S vs ----
II VS vs
vs vs vs vs
vs vs
vs vs
vs vs
vs vs
vs vs
vs vs
vs
vs
vs
vs
vs vs
vs vs
vs vs
vvss
vs vs
vs vs
vs vs
s VS
s vs
s vs
s vs
VS
vs
vs vs
s
ss
s
SS
s s ss
vs vs
vs vs
vs vs
<vs5.0
s
vs ss
VS vs
vs vs
vs vs
ss ss s SS
1
SS
s
5
vs vs
I
5160 25C
-- -- -- -- -- -- --
50 -- -- -- --
-- -- --
--
-- --
ll 0Z22U
TOWOLDMON0026632 WATER_PCB-00011101
FIG. 4
12
0222012
|
TOWOLDMON0026633 WATER_PCB-00011102
FIG. 5
vb^sal Seconds. o I I I
.U..n /
Sa y b o it
.
Viscosity,
Toxicity
Experimental work on animals shows that pro longed exposure to Aroclor vapors evolved at high temperatures or by repeated oral ingestion will lead to systemic toxic effects.
Repeated bodily contact with liquid Aroclors may lead to an acne-form skin eruption.
Suitable draft ventilation to control the vapors evolved at elevated temperatures, as well as pro tection by suitable garments from extensive bodily contact with liquid Aroclor*, should prevent any untoward effect.
Vaporization Loss
The Aroclors have low vaporization losses as shown in the data in Table I.
Estimated vapor pressures of several Aroclors ex trapolated from figure I are shown in Table VII.
TABLE VII
Approximate Vapor Pressures
Calculated at 100 F (37.8 C)
Aroclor 1232...............................0.005
Aroclor 1212...............................0.001 Aroclor 12 IH...............................0.00037 Aroclor 1251...............................0.00006
nun. llg.
mm. llg. mm. llg. mm. llg.
i:i
0
|
TOWOLDMON0026634 WATER_PCB-00011103
APPLICATIONS
Adh esives
'
TV heavier resinous Aroelors, liroaustr of their excellent adherence to smooth surfaces, arc very adaptable to compounding in water-insoluble adhesives. Aroelors 1260, 1262, 4465 and 5460 arc suggested ail constituents of compositions for this use.
Electrical Equipment
Because of 1 heir nonflammability, high resistivity and dielectric strength and low power factor, the liquid and resinous Aroelors are extremely useful materials for the electrical industry.
Aroclor 5160 is useful as an inipreguant for carbon radio resistors to reduce the influence of moisture. Since the liquid Aroelors will absorb sufficient moisture from the atmosphere to impair the elec trical characteristics, it is customer) to treat Aroclor intended for this application before use with a dehydrating clay. An effective product for this purpose is Attapulgus clay 80 800 mesh dried for 4 hours at 400C.and used at the rate of 0.125% based on the weight of Aroclor. followed by filtra tion. Treatment is improved if the Aroclor is healed to 80-85C.
Expansion Medium
Because of their stability under variations in temperature and freedom from gum formation from oxidation, the Aroelors are useful as expand ing media in bellows controls and in thermostats.
Hydraulic Medium
Power Transmission
The Aroelors arc superior hydraulic media for power transmission. Because of tlicir greater den sity and 1C. P. characteristics they approach more
closely the theoretical transmission values for mechanical power as illustrated in Figure 6. This greater efficiency makes possible a reduction in the size of the hydraulic coupling design.
In order to meet extremely low-temperature weather conditions, it is necessary to adjust the freezing point of the Aroclor selected by the addi tion of a pour point depressant. Suitable adjust ments can be made in the composition to reach a pour point of minus 65F.
The steepness of the viscosity-temperature curve of the Aroelors is a handicap to the application of Aroelors to many types of fluid transmission. This curve can be flattened to a marked degree by introduction of a viscosity-index corrector. By proper choice of viscosity modifiers and pour point depressants, the viscosity-temperature curve can be made to coincide with any standard hydro carbon oi! viscosity curve.
Information will be gladly furnished.
Hydraulic Pressure Medium It is customary to employ a D. T. Light Oil (mineral base) as a hydraulic medium in many types of pressure operations. A widespread use is in the operation of zinc-alloy die casting machines where pressures of 800 to 1500 pounds per square inch are encountered. Condensate from the atmosphere above the liquid level in the breather tank frequently introduces water, which, having a greater density, sinks to the bottom and is drawn into the system. Under the influence of heat and pressure the water causes oxidation of the hydrocarbon oil, forming fatty acids which corrode the pump vanes and the regulating valves of the system, causing loss of pressure, lowered production rate and final shut down for repairs. A break in the hydraulic system around the open flames necessary to maintain the molten condition of the dic-cusliug alloy almost invariably results in a fire with its attendant hazards.
Aroclor 1218 is recommended to overcome these difficulties. It is heavier than water, thus exclud ing it from the system. It is stable--not hydrolyzed
1 i
If
02 2201A
|
TOWOLDMON0026635 WATER_PCB-00011104
FIG. 6
ing circulating Aroclor through a water eoolcd heat exchanger, thus employing one medium for both heating and cooling.
. In special cases, Aroclors 1212 and 1254 can he substituted for the Aroelor 12 18. If extremely low outside temperatures are encountered, the less vis cous Aroelor 1242 can be used, but it has the disad vantage of being flammable above 330C (62CIi')-
iligher temperatures tip to 325C (617F) can be attained in the heating medium if Aroclor 1254 is used. Provision can easily he made for warm ing the Aroelor after a shut-down so that it can be pumped.
Design for a simple, effective liquid Aroelor heat ing system for small unit operations is available.
<f/V(5//V- SPtKO &PM.
under heat and pressure--and thus avoids corro sion and expensive delays for repairs. It is non flammable, thus adding to the safety of the oper ators and to continuity of production.
Gaskets Gaskets made from the usual types of material and synthetic rubber are unsuited for retaining Aroclors which have a swelling effect on such gaskets. Much more suitable arc gaskets made front noil-swelling elastomers such os Tluokol 1605-A (Thiokol Corporation) or Resistoflex 11*1001 (Uesislollcx Corporation).
Liquid Heating Medium Aroclors 1212, 12 IB and 1251 arc used as a circulating heating medium with great success. Good circulation and a well designed heating sys tem are necessary lo prevent local overheating ol the Aroclor heating medium. Aroelor 1218 is rec ommended for universal use up to 3I5C (COO0!') because of its fluidity at low temperatures ami its nonflammability.
In processes where a cooling cycle must also he introduced, provision cun he easily made for shunt
Lubrication
Air Compressors
The presence of oil, oil vapors or mixtures of oxvgcn and oil fractions in the discharge lines and receivers of air compressors presents a constant hazard which needs only a particle of hot carbon to create a serious explosion.
This problem has been solved hy engineers of one large user of this t>pe equipment by employing Aroclor 1251 as the internal lubricant for high compression air compressors. Their experience with more than 15 high-pressure compressors of various types is reported in the American Machinists' Magazine, September 28, ll) ll.
High Temperature
The heat-resisting, nonflammable characteristics of the Aroclors make them attractive as lubricants under conditions of high iem[M>r;<ture, as, for ex ample, in go\ernor s>Moms of central power sta tions. Aroclor 12 18 is well suited to this application. Straight Aroclor 1251 gave excellent results on a roller hearing lest operating at 255o-260Ql'' with much less carbonization or decomposition than the usual spindle oil under the same conditions.
15
0222015
TOWOLDMON0026636 WATER_PCB-00011105
Extreme Pressure
It is a well accepted hypothesis in the lubrication Industry that by the addition of certain elements such as chlorine, sulfur and others in the proper form to a lubricating oil, a certain chemical com* binalion takes place with the iron or steel metal bearing surfaces. These surface compositions tend to prevent seizure of the rubbing surfaces under extreme loads and under which loads, if the sole lubricant were a pure mineral oil, seizure or scor ing would result at once through film failure.
As an extreme pressure (E. P.) lubricant base added to a petroleum hydrocarbon oil in amounts up to approximately 15% by weight, Aroclors 1248 and 1254 materially increase the load-carry ing properties without reducing the viscosity of the resulting composition. These Aroclors repre sent one of the more adequate carriers for the element chlorine as an extreme pressure base, possessing the following advantages:
1. Stability. They are stable, even at higher temperatures, which permits neither separation of components nor appreciable change in physical or chemical properties during long periods of operation and should not cause continued chem ical action on metal parts except the particular chemical metal surface combination which is nec essary to effect high load-carrying capacities.
2. Non-volatile. Many other types of chlorine bearing compounds arc so volatile as to render them unfit for long periods of service because of the escape of the elements from the lubricant. The Aroclors are non-volatile at normal temperatures.
3. Non-oxidizing. Aroclors do not oxidize or thicken up to an objectionable degree.
4. A^n-corrostre. Aroclors are non-corrosive toward meta! surfaces.
5. Non-abrasive. Aroclors exert no abrasion on the machiucd surfaces.
6. Non-Uydrolysis. Aroclors do not hydrolyze in the presence of water, thus avoiding the genera tion of hydrochloric acid.
7. Compatibility. Aroclors are completely misci ble with mineral oils. 8. Color. Aroclors do not darken or change the color of the lubricating oil.
Submerged Lubrication
Under conditions of lubrication subjected to expo sure to water displacement such, for example, as lubrication of bridge rollers, a heavier-thanwater lubricant can be prepared from mixtures of Aroclor and oil, of which the following are typical examples:
Mix No.
*--% by Wt.-v Aroctor
Oil* 1248
Pour Point
Gravity at
15.5C
1 50 50
0F 1.1263
2 25 75 +5F 1.2703
Bright Stock: Gravity API 22*23
Approx. >b./gl,1 2
9.4 10.6
Viscosity 210 F--160 Saybolt Secs* Color ASTM--7-8 Flash Point--545F . Pour Point--15F
o i
10
TOWOLDMON0026637 WATER_PCB-00011106
SUGGESTED USES FOll AKOCEORS
tn
PLASTICS, PIGMENTS, LACQUERS, PAINTS ami VARNISHES
The Aroclors are compatible with most of the common plastics materials (sec compatibility table on this page). The degree of flexibility imparted by the Aroclors diminishes progressively in the order of liquid Aroclor -- soft resin -- hard resin. The hardness of the resulting compositions increases in the same order. Usually a satisfactory balance between flexibility and hardness can be obtained either by selecting the Aroclor of proper physical characteristics or by using a mixture of two or more Aroclors.
Ethyl Cellulose
The Aroclors are very compatible with ethyl cel* lulose, the liquids imparting great flexibility and the resinous products great hardness. 75 parts by weight of Aroclor 1212 with 100 parts of ethyl cellulose produces great flexibility and just a slight tackiness. Aroclor 5160 in the same propor tion produces a very bard and somewhat brittle composition. Aroclor 4165 produces hard films which are not brittle at ordinary temperature.
Compatibility With Various Materials
Asphalt............................................................... C
Benzyl Cellulose............................................... C
Cellulose Acetate............................................. I
Chlorinated Rubber........................................ C
Coumarone and Indene Resins..................... C
Dammar Resin................................................. C
Ester Gum......................................................... C
Ethyl Cellulose................................................. C
Manila Gum..................................................... I
Nitrocellulose.................................................... C
Paradm.......................................................
C
Phenolic Resins..............................................Varies.*
Polystyrene Resins.......................................... C
Rosin.................................................................. C
Rubber............................................................... C
Sulfur................................................................. C
Vinyl Resins..................................................... C
C-- Indicates compatibility to a degree sufficient to be of value.
I -- Indicates incompatibility.
* Not compatible in final stage.
For coatings of high gloss and exceptional weath ering qualities to be applied to rigid surfaces, compositions containing equal parts by weight of Aroclor 5460 and ethyl cellulose arc suggested. If greater flexibility is required, one of the softer Aroclors should be used, cither alone or as a replacement for part of the Aroclor 5160 and the proportion of Aroclor should be decreased.
A typical formula is as follows:
Ethyl Cellulose. ........................................ 15% Aroclor 1260.............................................. 5% Toluene....................................................... 56% Butanol...................................................... 14%
Graphic Arts
100%
The Aroclors are used as vehicles for carrying pigments employed in glass decoration. When the decorations have been applied and the glass is fired, the Aroclors volatilize without carboniza tion and thus avoid discoloration of the glass. Aroclors 1251 and 4165 are used.
Aroclor 4465 is a useful resin for compounding rotogravure inks.
17
TOWOLDMON0026638 WATER_PCB-00011107
A mimeograph ink suitable for use on bond pa|>or contains (lie follow ini' ingredients:
Aroclor 4165................................................ 40% Lubrication; Oil (SLV1200 (<i]00F).. 35%, Paraffin Oil (SLV 76 (5,100F)............ 20% Carbon Black............................................ 4% Oil Soluble Dye................. .................... 1%
Aroclor 4-105 may also be u&ed in the preparation of imitation gold leaf. A thin coating of the Aroclor is applied hot to one side of paper. While It is still hot, bronze powder is spread upon the coating. The bronze powder adheres to the Aroclor completely covering the paper. This product is U6cd in making the "gold leaf' letters on books, etc. The paper treated with Aroclor and bronze powder is placed upon the book binding. A hot die i6 pressed upon it. The Aroclor softens and sticks the bronze to the binding and forms a coat ing over it to protect it from tarnishing.
Impregnation
The Aroclors may be used to impregnate cloth, paper, wood or asbestos in order to impart mois ture and gas resistance, adhesion, insulating prop erties, Alkali or other chemical resistance, flame resistance, or lubricating qualities. For this type of work they are used in combinations with other materials such as waxes, inorganic pigments, asphalt, tars, aluminum stearate, sulphur, etc., in order to obtain exactly the phvsical character istics desired for the specific purpose. Aroclors 1251, 4165 and 5160, or the corresponding darkcolored products, arc suggested as most applicable.
Wood impregnated by vacuum-pressure method with the following mixture:
Aroclor 1165........................................ 70% M icrocrv stulliuc Wax...................... 20% Sulfur.."................................................. 10%
is definitely tougher,harder ami more moisture resistant than untreated woml. This coaling is very resistant to acids and alkalies but will be attacked l\ aromatic, aliphatic or chlorinated
hydrocarbons. The surface is not appreciably dis colored and can he painted. Various degrees of hardness and adhesion can he obtained by vary ing the Aroclor: wax: sulfur ratio.
Moisture Proofing
For use as moisture proof coatings tbc Aroclors are best combined with wax$s, such as paraflin or carnauba, oils such as mineral oil, and resins such as ester gum or other synthetic resins. The simplest compositions contain only Aroclor and paraflin. A moisture proofing compound composed of 96% (bv weight) of Aroclor 5460 and 4% of paraflin (melting point 54C) has an ASTM soft ening point of about 82 C and is very efficient. Substituting Aroclor 4465 for Aroclor 5460 pro duces a compound with a softening point of about 58C.
Softening point and viscosity when melted mav be further decreased by using mixtures of Aroclors. For example, a composition containing 40% of Aroclor 3260, 56% of Aroclor 5460 and 4% of paraflin will be very soft at ordinary temperatures. Increased proportions of paraflin will also pro duce softer compounds.
Pigment
Aroclor 1270 is a hard, white crystalline product of high inciting point, insoluble in most solvents, resistant to chemicals and to oxidation. When ground to a fine powder it makes an excellent organic pigment for use with the various plastics. It may be used alone or with conventional pigments.
Paints and Varnishes
The Aroclors arc soluble in paint and varnish oils and impart properties corresponding to the phys ical character of the particular Aroclor. The hard resinous Aroclors tend to give increased hardness to the Aims while the viscous resins impart flexibility.
!
022201B
|
TOWOLDMON0026639 WATER_PCB-00011108
The Aroclors do not react chemically with oils*
hence there is no advantage in heating together in
making a varnish. They arc best added as a "chili
back*' or as a cold cut in the thinning operation.
As far as incorporation of the Aroclors is con
cerned* the only reason for heating is to make
the Aroclors liquid so that they can he readily
mixed with the oils.
,
Aroclors 4465 and 5160 will produce paints that arc very quick drying and yet have excellent durability. The weight of Aroclor used should be from 30% to 50% of the weight of the oils.
Aroclor 1260 is best for short oil varnishes that are required at the same time to he flexible. The Aroclor may be considered to play the same role as oil, with the difference that it does not oxidize and lose its flexibility on exposure. Resins of the alkyd, phenolic or ester gum type* or a harder Aroclor such as 5460, may be used in making varnish formulations. It is suggested that for two parts by weight of oil, one part of Aroclor 1260 and one pari of oilier resin be used. These pro portions can be varied as required. The Aroclors impart water and alkali resistance and in these qualities enhance the value of the other resins used in the varnish.
Rubber and Rubber Substitutes
The Aroclors when in a liquid condition have a solvent action on rubber, both natural and syn thetic. Aroclors 1254 and 1260 are milled into ruhlwr in order to impart permanent tackiness and adhesion. A small amount of Aroclor 1260 added to hard rubber acts as a plasticizer and reduces the brittleness.
Aroclor 1270* being a hard crystalline material of high inching point* can be ground to a powder
and then milled into rubber. The milling tem perature being below the melting point of the Aroclor* the latter is disjiersed through the mass of rubber and acts as an efficient flame reducer. This same procedure can be used Vith synthetic rubbers to impart fireproofness. From 5% to 25% of Aroclor 1270 based on the weight of the resin is required.
Aroclor 1262 is recommended as a plasticizer for crepe rubber resin in paint compositions. Used in concentrations of 5% to 50%, based on the weight of the rubber resin, it increases the gloss and alkali resistance of the film and increases its adhesivcncss toward steel.
Aroclor imparts water resistance to Thiokol.
Modified Rubber Finishes
Aroclors 1242, 1251, 1260, and 1262 are recom mended as plasticizers for modified rubber finishes (chlorinated rubber* rubber hydrochloride and cyelicized rubber). Used in ratios of 5 to 50 Darts to each 100 parts by weight of modified rubber, they yield tough, flexible compositions, when used alone or in combinations with resins and oils. Resinous Aroclors 4-165 and 5460 used in the pro portion 50 to 100 parts to 100 parts of modified rubber yield harder films. The Aroclors arc espe cially valuable in compositions of modified rubber used as finishes for alkaline surfaces such as con crete* brick, stucco, etc. And as acid and alkiline coatings.
Vinyl Resins
The Aroclors arc compatible with all the vinyl resins and arc of value because of their chemical resistance. The properties imparted depend upon the particular Aroclor ami the vinyl resin used. The selection of the correct Aroclor for a particular use can usually he made by consideration of the physical properties of the Aroclor scries.
10
0222019
TOWOLDMON0026640 WATER_PCB-00011109
Nitrocellulose Coatings
The Arcclors function both as plasticizer* ami resins ami may be used aUme with the nitro cellulose or in combinations witlc oilier plasti cizers or resins. They impart weather resistance, luster, adhesion and decreased burning rate. Their excellent electrical characteristics (high dielectric strength and rcsistmt\ and low power factor) ami their property of retarding the passage of moisture and gases through nitrocellulose, chlorinated rub ber, and other similar plasties films make the Aroclors of sj>ceial value in coalings for electrical insulating materials.
The accompanying trilincar diagrams show the practical compatibility limits of Aroclors 125-1 and 1262 when used in conjunction with some other resins and plasticizers. Aroolor 1260 gives values almost the same as those shown for 1262. The less viscous Aroclors have greater and the more res inous Aroclors less compatibility than for those shown. (See trilincar diagrams that follow.)
To illustrate the differences possible to obtain
by changes in formulation, three formulas are given below. All have excellent durability but the third is much softer and more flexible than the other two. Only the solids contents are given.
The amounts tubulated are parts by weight.
Aroclor Lacquers
No. 1 ^second Nitrocellulose (dry]1 100 Danunar resin........................ , 80 Ester Gum..............................., -- Aroclor 1260........................... 20-39 Dibulyl Phthalate..................20- 0 Tricrcsyl Phosphate.............. --
No. 2 100 -- 80 20 20
~
No. 3 100
--
--
80-70 --
39-70
No. 1 and No. 2 have excellent sanding and polishing qualities. No. 3 is very flexible but too soft for sanding. Where extremely high flexibility is desired, as for example in lacquers for high tension automotive cables, the following composition is suggested: 15 -- 20 sec. R. S. Nitrocellulose......................... 100 parts by weight Tricrcsyl Phosphate............. 120 parts by weight Aroclor 1242.......................... 80 parts by weight
o
20
0232020
TOWOLDMON0026641 WATER_PCB-00011110
DIAGRAMS SHOWING PRACTICAL COMPOSITION
OF LACQUKHS USING AROCLORS 1251 AND 1202
In the trilincar diagrams the compositions, represented by any point in the unshaded areas, arc those which produce homogeneous lacquer films. On the other hand compositions represented by points in the shaded areas produce impractical, segregated, brittle or soft films. For detailed information as to the derivation and use of these diagrams reference is made to the following articles:
Jenkins & Foster, "Compatibility Relationships of the Aroclors in Nitrocellulose Lacquers," Ind. Eng. Chem. 23, 1362 (1931).
Hofmann & Reid, ''Graphical Methods in Lacquer Technology." Ind. Eng. Chem. 20,431 (1928); "Formulation of Nitrocellulose Lacquers," Ind. Eng. Chem. 20, 68? (1928).
0222021
|
TOWOLDMON0026642 WATER_PCB-00011111
Israel leal <0.11|mn!l ii of Liif`i|iiors using
Arorlors 1254 ami 12<2 -- ((ontinuiul^
plillmlic anhydride-glycerol type and where the Aroelor is Aroclor 1262.* Aroclor 1260 may lie aubatilutcfl without material change.
22
TOWOLDMON0026643 WATER_PCB-00011112
Aroclnr 1262* And where the plasticizer is Tricrenvl Phosphate.
0Z^*3
|
TOWOLDMON0026644 WATER_PCB-00011113
The information contained in this booklet is to our best knowledge true and accurate, but all recommendations or suggestions are made with* out guarantee, since the conditions of use are beyond our control. Monsanto Chemical Company disclaims any liability incurred in con nection with the use of these data or suggestions.
Furthermore, nothing contained herein shall be construed as a recommendation to use any product in conflict with existing patents cover ing any material or its use.
Monsanto Chemical Company St. Louis
PL -47-7I
24
PRINTED IN U. 8. A.
TOWOLDMON0026645 WATER_PCB-00011114