Document pmbqMRjObqkQD65vaGaBbp126
Monsanto
&FROM (NAME LOCATION)
,'
C. D. Bias - St. Louis Organic Research
OATE
:
SUBJECT
:
REFERENCE
:
TO :
May 12, 1969
cc: M. W. Farrar
Res. I
J. R. Darby
.
Res. :
United Resins/Bacon Packaging
W. F. Waychoff
WWAYC
J. K. Lilly
JLILL
Work Request 69-21
C. P. Farley/P. R. Graham CFAI
W. E. Schalk
WSCHA
Cumming Paton
J. A. Cannon
Res. ;
CPATO
P"#1,j A
Ka
u'
^^r7W.:M;:;T2oaker:;?!-^ R. H. Mills
N. W. Touchette
Res. ; Res. ;
You have asked that we take a quick look at the samples of bacon packaging hot melt which United Resins has picked up from a competitor. You indicated that five different suppliers have analyzed the hot melt and that United now has five different results. We can now probably add another, so they will have six.
Our results confirm that it does indeed start to melt at around l8o F and smokes at 290 F. None of the formula tions which we tried melted or smoked quite so low. ^
We prepared several different formulations, using United's suggesting, and varying it slightly. We also included some Aroclor samples for comparison. | The hot melts were heated in an oven, mixed thoroughly, f&nd poured onto a
plate so that films could be drawn down for subsequent tensile testing. Formulations used and results are:
1 2345 67
Competitive hot melt
100
Elvax 260
24 24 20
Be Square Wax 190
28 36 32
Piccolyte S-70
48 40 48
ARoclor 5^60
24 24 28 36
20 32
48 40 48
Elongation, $ 100$ Modulus, PSI Tensile Strength, PSI Toughness
355 690
1040
8.4
370 360 380
4.8
150 420 420
2.3
195 390 380
2.4
495 510
1170 12.1
425 560 910
13.5
445
590 1100
12
Piccolyte S-70 seems to have a detrimental effect on tensile strength in the concentrations used. Also, from observa tion of the hot melt, there appears to be significantly more wax present than formula #2 indicates. If Piccolyte S-70 is actually the modifier being used, then we would suggest that the competitive formula is something on the order of 40$ Elvax 260, 40$ wax and 20$ Piccolyte S-70.' It may be
DSW 587539
t
STLCOPCB4092875
Cuming Paton March 12, 1969 Page 2
that the wax used is a much lower melting one than what we used, perhaps even a paraffinic oil. If so, that would explain the excessive smoking and lower melting of the competitive product. As agreed by telephone, we will not pursue this work any further at this time.
C. D. Bias
JP
n
A-
I
DSW 587540
STLCOPCB4092876