Document pDj4K0EVJm8OzXMXm2KMn1oD

/ Monsanto MONSANTO TRADE LITERATUjX PERMANENT FILE . 8 _ AROCLORji Chemicals--Plastics 3or Poly.viny.1 Acetate Lmuliion crfdkeiivei Monsanto Tochnical Bulletin No. 0-111 November, 19S5 ______ __________JL Monsanto Chemical Company, Organic Chomicals Division, St. Louis 1, Mo. INTRODUCTION Monsanto Aroelor* chlorinated polyphenyls are a series of compounds serving a variety of needs. Each Aroelor can serve as a plasticizer for many of the synthetic resins. Properties imparled vary with the Aroelor chosen. In this respect the family of Aroelor compounds is analogous to a series of phthalate esters. Aroelor 1221, 1232 and 1242 are three compounds especially suited for plasticizing polyvinyl acetate (PVA) emulsion adhesives. ** These are important advantages of the Aroelor plasticizers specified -- 1)... Excellent tack and strong bonding power are imparted to PVA adhesives. 2) The compounds are low in cost. 3) The plasticizers are light colored. 4) Aroelor 1221, 1232 and 1242 are mobile liquids at room temperature. Plant handling is simplified since no pre-melting is required. 5) The plasticizers are readily blended with PVA emulsions by simple stirring. 6) The hardness desired In various adhesive applications can be varied by - choice of Aroelor plasticizer without materially changing other properties of the adhesive. 7) The three Aroelor plasticizers recommended for PVA emulsion adhesives are comparable to or/Ao-Nltrobiphenyl (a widely used PVA plasticizer), with regard to tack and fiber-tear, as indicated by tests on a porous yellow paper and a melamine-coated Kraft stock. 8) Aroelor compounds are readily available. > o i. tm- o. a hi. w. TW ifll, < will, MOMS 080417 COMPATIBILITY Tests comhictcd by Monsanto show Aroclor 1221, 1232 and 12^2 are each compatible with PVA at the evalua tion level of 11 parts of plasticizer in 100 parts of polyvinyl acetate emulsion. Each of the Aroclor plasticizers will blend with nrf/to-Nnrobiphenyl, if blending is desirable. Add liquified ONB to the emulsion, then add the Arorior. LABORATORY DATA Several l'VA adhesive formulations using different plasticizers were made up and evaluated in our laboratories. The basic formulation consisted of 11 parts of plasticizer in 100 parts of polyvinyl acetate emulsion. Data tabu lated below will allow the adhesive fortnulator to choose the most suitable plasticizer for the adhesive proper ties desired. A COMPARISON OF POLYVINYL ACETATE PLASTICIZERS Formulation Properties ortho-NItrp- Dibutyl 'biphanyl Phthalata Aroclor 1221 Aroclor 1232 Aroclor 1242 Short Hardnaw, A-scale 82 69 66 86 97 Low Tamp. Fits., C. + 2.2 -10.2 -- 5.9 +4.0 + 5.3 Volatility plasticizer lost after 2'4 hrs. at 86 C.) 3.8% 4.0% 4.8% 4.3% 4.0% Kerosene Extraction, (% plasticizer lost after 24 hrs. at room temperature) 3.2% 4.1% 4.5% Viscosity of Formulation* (Centlpolaes) Initial 1 day 3 days 4 days 5 days 7 days 10 days 2160 -- 2200 -- 2280 2340 246Q. , 2420 2460 -- 2520 -- -- .... 2240 __ 2200 __ 2200 2180 2260 viKD>i<y of the polyvinyl cette tmultion tested wu \ 500 centipoiiet. 3.8% 4.2% __2160 __ __ 2060 __ __.... 2040 __ 2020 __ 2060 .... -2MUNb 000410 1 L TYPICAL PROPERTIES AND SPECIFICATIONS Property Arocior ,, 1221 Arocior 1232 Arocior 1242 Color, APHA max. (Specification) Acidity, max. (mg. KOH/gm.) Specific Gravity, 25/15.5 C. (Specification) Pounds Per Gallon Distillation Range*, 0 C. Flash Point, C.O.C., 0 C. . , F* Flro Point, C.O.C., C. F. Poor Point, ASTM-D-97, 0 C. Refractive Index, nD** Viscosity, S.U.S. 210 F. (ASTM-D-88) 130" F. (Specification): 100 F. ASTM'D'IO (modified). 100- 100 100 0.014 1.182-1.192 0.014 1.270-1.280 0.015 1.381-1.392 9.85 275-320 50 286-302 176 349 Crystal* at 1 1.615-1.616 ' 10.55 295M550 149-152 300-305 ju 415 --35.5 TS18-1.620 (Specification) 30-31 35-37 38-41 ' 31-32 39-41 44-51 **No fire point up to boiling temperature. 11.50 325-360 176-180P 348-356 None** -- -19 1.624-1.626 (Specification) 34-35 49-56 82-92 TOXICITY AND SAFE HANDLING INFORMATION /./s> /.V ' The acute oral toxicity of Arocior 1242 abows U to have an LDM to rets of 4.15 ml./kitogram. Presumably the other two Arocior compound! are in the same toxicity range. Repeated or prolonged skin contact with these compounds is to be avoided. Inasmuch as their processing in this use does not require the use of elevated temperatures, there should be no hasard from vapor exposure. SHIPPING INFORMATION Shipping Classification (U.S.A.) Shipping Regulations Standard Containers --Synthetic Resin --None -- 55 gal. black iron, nonretumable, lacquer-lined drums containing 500 lbs., net, (Arocior 1221 and 1232) or 600 lbs., net, (Arocior 1242). -3HONS OaO<tl9 l A ROCLOR 1221, 1232, and 1242 For Polyvinyl Aeotafo Emolsion Adheaivef Monsanto Chemicals "Plastics _______ ___________ _ *>* tw to liM SuSaHn Ho. 0-1 n Wm h i B i i , IMS For luHkor hfomailvA on tin proJooH ^mrlM In this buMotin eoflttd fbo amiw( Monsanto offkw. MONSANTO CHEMICAL COMPANY ST. LOUIS AKRON ATLANTA BOSTON CHICAGO CINCINNATI CLEVELAND DETROIT HOUSTON LOS ANGELES MINNEAPOLIS NEW YORK SAN FRANCISCO SEATTLE WILMINGTON MONSANTO CHEMICALS LTD. London MONSANTO CHEMICALS (AUSTRALIA) LTD. Molboumo MONSANTO (CANADA) LTD. Montrool Toronto Vancouvor Rapraaonfativaa in tha Principal Citiaa of the World MONS OBOAdO