Document nNw1e43J2rBZvkGk4oOQNKx8

Handbook ASBESTOS TEXTILES THIRD EDITION YfcTyl ASBESTOS TEXTILE INSTITUTE FOUNDED 1 9-4-4 CONTENTS Pagi Introduction'........................................................................................... vii The Mineral Asbestos............................................................................ 1 The Mining, Milling and Grading of Asbestos Fibers 15 Processing Asbestos Textiles...............................................................24 Asbestos Textile Products.................................................................... 29 Asbestos Lap......................................................... ... 34 Asbestos Roving........................................................................... 36 Asbestos Yarn........................................................................... 38 Asbestos Cord 40 Asbestos Thread................................................................................41 Asbestos Cloth................................................................................42 > Asbestos Tape................................................................................48 Asbestos Tubing................................................................................52 Asbestos Wick................................................................................54 Asbestos Rope 55 Non-Woven Asbestos Felts...............................................................57 Carded Asbestos Fiber . . 58 t ASTM Specifications and Methods of Testlng.................................. 60 Glossary................................................................................................. g7 ......................................................................................................10i v Asbestos Textile Institite 1967 Litho ix U.S.A. Libbabv of Congress Cataloc Caro Nimber 66-30393 Price $1.50 per copy TO THE MEMORY OF DR. MYRIL C. SHAW WHO SERVED AS EXECUTIVE SECRETARY OF THE ASBESTOS TEXTILE INSTITUTE FROM 1948 TO 1963 AND WHOSE WORK AS RESEARCH FELLOW CONTRIBUTED IN COUNTLESS WAYS TO THE ADVANCEMENT OF THE ASBESTOS TEXTILE INDUSTRY From the mineral asbestos, hard and rocklikc in structure, come the soft, silky fibers that arc made into many forms of textile products i 4 rocklike 'r* that products INTRODUCTION Legend tells us that the Emperor Charlemagne delighted to mystify his dinner quests bv throwing an asbestos tablecloth into a roaring fire and then removing it. unharmed, from the flames. Thus was demonstrated, more than eleven hundred vears ago, one of the outstanding characteristics of textiles made from the fibers of that re markable mineral, asbestos. Todav. the products which come from the cards, spinning frames and looms of asbestos textile manufacturers constitute a virtually indis pensable part of our modern industrial economy. In the electrical industrv. for example, asbestos textiles meet the special requirements of an efficient insulation for wires and cables. As such, they are widely used in ranges, refrigerators and other home appliances, as well as in industrial furnaces, ovens, welding machines, motors and transformers. They are a basic component of mechanical packings and j gaskets. Thev assure the stamina and heat resistance so essential in autoj motive and industrial friction materials, gears, bushings, bearings and ! other vital mechanical parts. Impregnated with resins and ceramics, asbestos textiles increase the strength and durability of numerous products. In one of their newer ap plications in this form, they serve as thermal insulation in the nose cones, fins, combustion chambers and other areas of missiles and rockets where temperatures in excess of 5000 F are encountered. Asbestos textiles are also found in such widely diversified uses as safety clothing, fire-smothering blankets, conveyor belts, filter cloths, fireproof curtains and draperies, and as thermal insulation for exhaust pipes. In fact, there is scarcely a major industry' or activity' that does not benefit 1 in some way from the use of asbestos textiles. They have raised safety' standards, improved product performance, lowered costs and contributed 1 other important advantages in numerous fields--and their range of use fulness is ev er-increasing. vii t Serpentine rock with veins of chrysotile asbestos fibers as they appear before separation The Mineral Asbestos Asbestos is the name given to a group of fibrous minerals that o in different forms in many countries throughout the world. The wot derived from the ancient Greek language and its first recorded use by the Roman naturalist, Pliny the Elder, in the first century A. although asbestos itself was known to the Greeks and used by ther an even earlier date. Early in the first century', the Greek geographer Strabo referred to a st from southern Greece that was carded and woven into handkerchi "Karystos lithos," the Greeks called it, naming it after the city wher was found. The Romans had also developed uses for this amazing stone it is known that they wove it into lamp wicks and cremation cloth wrapping their dead. And that famous Venetian traveler Marco Polo, he from wandering in Siberia in the thirteenth century, brought news c "fossil substance" which, "when woven into cloth and thrown into the f remains incombustible." He, too, had become acquainted with asbesl These early uses were of minor significance, however, and it was not ui the advent of the steam engine, with its need for insulation and pack that asbestos really began to assume commercial importance. The ni: teenth century saw the discover)' of large deposits in Canada and Soi 1 Africa and todav asbestos is one of modem man's most important raw materials. As a component in an uncounted number of essential products, it is virtually indispensable to us in our everyday living. MAJOR PROPERTIES The commercial value of asbestos depends largely on two physical char acteristics -- its incombustibility and its unique fibrous structure. The latter permits it to be separated into filaments or fibers, many of which possess high tensile strength and unusual flexibility and are adaptable to numer ous uses. Some tvpes of asbestos can be spun into yarn and woven into cloth and are thus the basic raw materials from which asbestos textiles are made. Other valuable properties of asbestos are its resistance to heat, moisture and corrosion. However, these properties, like some of those already men tioned, are found to vary considerable with the different types of asbestos and, to a lesser extent, between diilerent specimens of the same mineral. Tables 13 and C, pages b and 9, provide an interesting comparison of the properties of several varieties of asbestos. VARIETIES OF ASBESTOS Some thirty or more minerals of fibrous crystalline structure comprise the asbestiform group but only six have economic significance. These are, in order of importance, chrysotile, crocidolite, amosite, anthophyllite, tremolite and actinolite. Chrysotile is a fibrous form of serpentine; the other five are amphiboles. Because it is superior to other types of asbestos for textile processing, as well as for industrial purposes generally, chrysotile accounts for about 95 per cent of the total world production of natural mineral fibers.1 Chrysotile asbestos fibers after separation from the mother rock. The fibers have been pulled apart to disclose their fine silky nature .mt raw roducts. al char ge latter possess numerven into .tiles are noisture dy men'.sbestos mineral, n of the rise the are, in . tremoie other sing, as bout 95 rs.1 ''sbestos potation <r rock. e been disclose ' nature CHRYSOTILE Chrvsotile is a hydrated magnesium silicate having an empirical formula which, in the past, has often been expressed as 3MgO-2SiO;>.2HoO. How ever, recent studies of the structure of chrvsotile show that all the water in the composition exists as hydroxyl (OH-) ions. Thus, the empirical formula is perhaps more correctly expressed as Mgs^OH^Si^O.-,] or a multiple thereof to show the actual state of the water in the structure. Origin: Almost all of the world's resources of chrvsotile asbestos are asso ciated w ith ultrabasie igneous rocks which were injected into the earth's crust. A prerequisite to the formation of asbestos was the hydrothermal alteration or rock metamorphism of the crystalline ultrabasie rocks to amorphous serpentine. Equally important in the asbestos formation process were the structural deformations which produced wide scale frac turing within the solid serpentine mass, permitting the entry and circu lation of siliceous solutions. A number of hvpotheses have been advanced to explain the actual manner of asbestos formation. The most acceptable of these is that the siliceous solutions entered the fractures within the serpentine mass under condi tions of high temperature and pressure. Over a period of time magnesium silicate was dissolved from the adjacent rock. Gradually, both the tem perature and pressure moderated such that the solutions became super saturated with magnesium silicate and crystallization took place in the form of fibrous asbestos. The asbestos fibers grew in a direction normal to the fracture and the iron released during the process was deposited as magnetite. Nature has exercised some variety in the formation of chrysotile, as is apparent by the fact that "impurities" in the crystal structure are the rule, not the exception. An example is the presence of atoms of iron re placing magnesium in the crystal lattice. Such replacement is quite vari able. Other elements are also present. These include traces of calcium, aluminum and other elements in amounts so small that they are disclosed only bv spectrographic analyses. Magnetite and, to a lesser extent, chro mite are found frequently K ing between the serpentine and the vein of chrysotile and consequently small pieces may be found in fiberized chryso tile. But despite these variations, chrysotile is generally more uniform in quality than other types of asbestos. Properties: The properties of chrysotile fibers which particularly adapt them to the manufacture of asbestos textiles are length, strength, tough ness, flexibility or pliability and a minimum of magnetic or conductive 1 Asbestos -- A Materials Survey, U. S. Dept, of the Interior, Bureau of Mines, 1959. 3 particles. Chrvsotilc fibe rs are the most flexible of am asbestos fibers. Their tensile strength is hitjb. and individual values of more than bOO.OOO psi have been recorded. How ev er, the measured tensile strengths of a series of fiber bundles tend to show variations as a function of length. Although rare specimens of chrvsotilc have been found up to several inches in length, commercial fiber ramies downward from three-quarters of an inch. In general, onlv the longest av ailable fibers arc used in the process ing of textiles. See 'Textile Grades, pane 20. Resistance to Heat: Chrvsotilc rates high aiming the asbestos minerals in resistance to destruction In beat. I'nder continuous and long expo sures. there is loss of a small part of the structural water in the fiber at 750: F and at 1110 F most of the structural w ater is lost. Fusion occurs at 2770: F. However, under transient conditions and those short of equilibrium, chrvsotilc will retain its structure over a much higher tem perature ramie. Practical examples of this are found in numerous high temperature applications where the fibers, in combination with other materials, successfullv withstand exposure to temperatures as high as 6000= F. Recent studies of chrvsotile asbestos by means of the electron microscope and gas adsorption and desorption isotherms show that the fibers are tubular in structure but with the fiber pores generallv filled or blocked with an amorphous material of the same chemical composition. The struc ture of the fiber consists of las ers of silica and magnesium hydroxide with the hydroxvl on the exterior surface. This accounts for the unique hydrous characteristics exhibited by chrysotile. Spinnability: The better grades of chrvsotile are noted for their extreme fineness or silkiness which, together with their exceptional flexibility and high tensile strength, results in superior spinnability. Chrysotile may be subdiv ided into ultimate fibrils so fine that they are rev ealed only with an electron microscope. The diameters of these minute fibrils appear to be in the range of 200A to 400A (1A=0.0000000039 in.). This is many times smaller than the diameters of other commercial fibers. See Table G, page 11. The crude chrysotile from different localities is, however, variable in yield ing to the fiberizing process, the types which are easily fiberized being in general the finest, strongest and silkiest fibers. Fibers from different sources have distinctive, characteristic "working" properties. Chrysotile may be soft and unctuous to the touch, or it may be somewhat harsh. Harshness, which generally is accompanied by' a lack of optimum pliability, resists fiberizing and requires more time in processing. 4 Ms fibers. Tlicir .in Sl)O.(KH) psi i' of a scries of `-Z111. Although . ml indies in carters of an ; ihc proccss- niincrals Hi long espon the fiber at fusion occurs i.ose short of lowlier tem- illKTUIIS high i with other s as 3iicili as a microscope iie fibers are il or blocked >n. The strueydroxidc with aique hvdrous - heir extreme dexibilitv and otile may be only with an 's appear to ,rhis is many "-o Table C, `hie in yield'cd being in ' working" ,r if may be ' ;i I n k of i'r"',Ssi,,g. j r''' rusotile asbestos ; rv as seen tinder ' I'lrctron rniernat approxi:>: it/ 40.000 maz- :: mrations. Thor :.<n!ar structure is ronarent from the 'jilt lines running .. 'cii the center of most of the individ ual fibers When harshness is accompanied by brittleness the fiber may be unsuitable for textile processing. These objectionable properties may be found in ehrvsotile derived from both igneous and sedimentary formations--in mas sive serpentine or in tabular bodies of serpentinized dolomite. They are not peculiar to either. But in the ehrvsotile of Arizona there are degrees of harshness, including 'semi-harsh." Semi-harsh chrysotile requires a special technique to make it suitable for textile use. The knowledge of these things that may impair the quality of chrysotile is a part of the know-how gained through experience and possessed by the personnel of the producing organizations in the asbestos textile industry. Sources: Chrysotile, most important of the natural mineral fibers, is for tunately also the most abundant of those having commercial value. It occurs in many countries but Canadian and African deposits are the major sources of the fiber that support the American asbestos textile industry. In Canada, Quebec has long been the principal source of chrysotile, al though extensive deposits are also mined in Newfoundland and British Columbia. Canadian output amounted to 1,416,650 short tons in 1964-, a major portion of the total free world production of asbestos fiber. In its crude rock form, Canadian chrysotile usually has a dark green luster, but the fibers appear white when fully opened. For this reason, it is known in the trade as "white asbestos." The British Columbia chrysotile, valued for its low magnetic iron content, is particularly well adapted for use as electrical insulation. - U. S. Dept, of the Interior, Bureau of Mines Minerals Yearbook, 1964. 5 _J : .1 1.1., . Other important suppliers of chrysotile fiber include Rhodesia, which produced approximately 153.000 short tons in 1964:!, and the United States, with a production of 101.092" short tons during the same year. The "soft" iron-free variety of Arizona fiber is particularly suitable for elec trical insulation but little has been available in recent years. Chrysotile is also produced in substantial tonnages in Italy, Swaziland and the Union of South Africa and in smaller amounts in Cyprus, Japan, Yugoslavia and other countries. Among Communist countries Russia is the leading producer, with an estimated production of 1,300,000 short tons in 1964.3 OTHER TYPES OF ASBESTOS Croeidolite: An amphibole of the hornblende group, crocidolite is the blue asbestos of commerce. It is a complex silicate of iron, magnesium and sodium corresponding approximately to the chemical formula XaoMgFe,-, [ (OHjSi^Oj 2 ]2. Its composition, like that of chrysotile is found to vary. Crocidolite is more difficult to process into a spinnable fiber than chryso tile, although some yarns and other textile products are made of this fiber. Crocidolite is also used in the form of mat, ro\'ing or as dispersed fiber as a reinforcement for plastics, particularly where high chemical resistance is required. Its resistance to heat is lower than that of chryso tile but its tensile strength is generally very high, a maximum of 876,000 psi having been recorded. The most important advantage of crocidolite is its superior resistance to attack by acids. The major sources of crocidolite are the Cape and Transvaal Provinces of South Africa, which produced nearly 103,000 short tons in 19643. De posits also exist in Australia and Bolivia. Because of its low strength, the soft silky' Bolivian crocidolite falls just short of being a textile fiber. It has good dielectric properties and is suitable for felting. Amosite: Also a fibrous amphibole, amosite -- MgFeG[(OH)Si.i011]2 -- is essentially a ferrous silicate in which a proportion of the iron is replaced by magnesium. The ratio of magnesium to iron may vary and minor replacement of the main components by other elements may also occur. Amosite possesses good tensile strength and is more resistant to heat than chrysotile or crocidolite. Its fibers are flexible and unusually long and al though not well adapted to spinning because of their relative harshness, they are well suited for the production of non-woven textile fabrics for 3 U. S. Dept, of the Interior, Bureau of Mines Minerals Yearbook, 1964. 6 i dcsia, which the United ne year. The ble for elec- Swaziland prus. Japan, es Russia is X) short tons lolite is the magnesium ,al formula hrysotile is han chrysoade of this is dispersed ;h chemical t of chrysoi of 876,000 crocidolite 1 Provinces 19643. Derength, the iber. It has is replaced and minor also occur. ' heat than ng and alharshness, "abrics for V reinforcement of plastics and of bonded and unbonded felts and batts for fire protection applications. Long fiber amosite is used principally in the manufacture of thermal insulation. Deposits located in Transvaal Province, Union of South Africa, provide the onlv commercial source of amosite fiber. Approximately 77,000 short tons were produced there in 19643. Anthophvllite: Essentiallv a silicate of magnesium and iron, usually with a small amount of aluminum, anthophvllite belongs to the group of orthor hombic amphiboles. Its chemical formula may be expressed as (Mg,Fe)7 [(OH^LOuJo. The fibers of anthophvllite are usually brittle and lack ing in tensile strength and are therefore not suitable for textiles. Tremolite and Actinolite: These monoclinic amphiboles are least im portant of the commercially used varieties of asbestos. Tremolite -- Ca2Mg.-, [(OH)Si40! j ]2 -- is a calcium-magnesium silicate whose fibers are often long and silkv but generally too brittle and of in adequate tensile strength for use in the fabrication of textiles. It is of value principally for filtration purposes because of its freedom from iron and its resistance to attack by acids. Most of the tremolite fiber produced comes from deposits located in northern Italy. Actinolite -- Ca2 (Mg,Fe)c [(OH )Si^Oj x]2 -- is similar in composition to tremolite except for the presence of iron which replaces some of the mag nesium. The fibers are too weak and brittle for spinning but have good resistance to acids. Its practical value is limited and production is small. TABLE A--CHEMICAL COMPOSITION OF VARIOUS TYPES OF ASBESTOS* Chrysotile -- Crocidolite Amosite Anthophylute Tremolite SiOo ............ MgO ............ FeO .............. FcoOa .......... Al->03 H-0.............. CaO .............. Na20 ............ CaO+NajO . 37447c 39447c 0.0-6.07c 0.1-5.07o 0.2-l.S7c 12.015.07c Tr.-5.07o 49-537c 037c 13-207c 17-207c 2.54.57c 4.0-8.57) 49-53% 1-7% 3444% 2-9%, 2-57, 56-58% 28347c 3-12% 0.5-1.57c 1.0-6.07: 0.5-2.5% 51-627) 0-30% 13-5.07, 1.04.0%, 0-5.07c 0-18%, 0-9%, Encyclopedia of Chemical Technology, Vol. 2--Anthrone to Carbon Copyright 1948. Inlerscience Publisher, New York and London. c/: C/2 u c/2 td 5 u i A- Canadian M ining and Metallurgical Bulletin, A p ril, 1951 t i l . Zukowski and II. Core. Nature, IH.'t, 35 (1959) 9 Cancdtfft M in in * and M etallurgical BuIJrfin, A pril, 1951 tA recently ilrtennim*<l TABLE D--EFFECT OF TEMPERATURE ON LOSS IN WEIGHT OF ASBESTOS FIBERS* 1 emp. r : 1IME Loss In Weight (Per Cent) Amosite Amhopmvllite CiirysotilejCrocidoute iTremolite 400 600 700 800 900 1000 1100 1200 1400 2 hrs. ** " i i *' " i i 0.23 0.57 0.80 0.98 LOT 1.16 1.36 j 1.39 ! 1.43 | 0.05 0.24 0.30 0.38 041 0.44 0.52 0.54 0.54 0.30 0.85 1.78 2.17 283 3.99 ( 10.38 I 12.75 1 13.43 | j 1 | 0.08 0.25 0.49 0.73 0.83 0.86 1.00 1.04 1.03 0.04 0.08 0.13 0.22 0.26 0.29 0.37 0.37 0.47 'Canadian Minins and Metallurgical Bulletin, April, 1951 TABLE E--COMPARISON OF SURFACE AREA OF VARIOUS FIBERS WITH ASBESTOS* Type of Fiber >i rtack Arm b\ .V. Adsorption <Sq. Cm./Gram) Silk ................................................................................... Asbestos <Chrvsolile) .................................................... 3.100 3.800 7,200 7.600 9.600 9.800 130.000 to 220,000+ 'Canadian Minins and Metallurgical Bulletin, April, 1951 +Recent studies show that the maximum surface area may run as high as 500,000 sq. cm./gram TABLE F--COMPARISON OF TENSILE STRENGTHS OF VARIOUS FIBERS* Type of Fiber Tensile Strencth ipsi) Maximum Acetate Rayon ................................................... Nvlon ................................................................... Class .......................................................... Orion ........................................................ Cotton ....................................................... Silk ........................................................... Wool ................................. Asbestos (Chrvsotile) ........................ 23,000 to 30,000+ 80,000 to 117,000+ 315,000 80,000 125,000 83,000 28,000 824,0001 'Tests conducted by Harris Research Laboratories, Washington, D. C., except where noted +Depending on type 1R. Zukowski and R. Care, Nature, 183, 35 (1959) 10 T\BLL C--COMPARISON OF DIAMETERS OF VARlOls FIBERS WITH ASBESTOS* Tel of Fiber ilumjn Hair : i JJTlitr ... '.....I ....... * . I:"n .... iIjn .-n ........ \A|..!I ......... iuu w.v.r Fibih Diameter i 1NCHLS 0.00158 0.0O0985 IMII'OH to O.0011 o.ooo; o.ooo.'i lEOOOl 0.o0u26 o.O'iolIJ 1" 0.000281 O.UOOOOOT06 i.i 0.00000118 (.jiuJian Mining and Metallurgical Bulletin, April, 1951 Fibrils in One Linear Inch 630 1.015 910 K. 12150 2.500 3.300 3.300 3.810 3.520 7.010 850.000 lu 1,400.000 TABLE H--EFFECT OF HEAT ON TENSILE STRENGTH OF CANADIAN CHRVSOTILE CHIDE* TiN'ILL MKENCTH * PSf < : iiti*--- \cr if-ar - at If 1 F .......... il-aN-o . at Hi it) F .......... ll.-jteu . > minutr r at 1000 F .......... 11 eult'i 1 t nunnlf - at 1200 F .......... 1 131.000 120.OO0 96.0*30 78.000 42.000 Canadian Mining ami Metallurgical Bulletin. April. 1951 Per Cent of Original Tensile Strength 91.6 73.3 39.5 32.0 TABLE J--COMBLSTION ANALYSIS OF CHRVSOTILE ASBESTOS* ------------------------------ -------1 Source or Fiblr ;Temp K Per Cent ; H;0 Arizona ........ 1000 1800 3.37 12.89 Per Cent CO,. 0.54 1.91 Total Per Cent Per Cent Icnition HM3+ Loss OF co,. Fiber 3.91 14.80 3.87 14.80 COg Cal ;t LATtD in Teh MS OF Percent ACE OF MgCOa CaCOn 1.03 -- 1.03 3.11 Australian ... 1000 1800 1.50 12.48 0.66 0.96 2.16 13.44 2.06 13.33 1.26 1.26 -- 0.68 Canadian <A) 1000 1800 1000 1800 5.47 14.28 1.82 12.00 0.85 0.97 2.54 2.89 6.32 15.25 4.36 14.89 6.23 15.17 4.28 14.84 1.62 1.62 4.85 4.85 -- 0.2* -- 0.79 Canadian <Bj 1000 1800 3.75 13.31 0.45 0.48 4.20 13.79 4.14 13.75 0.86 0.86 -- 0.0. 1000 1.98 0.77 2.75 1800 11.74 1.06 12.80 Canadian (C) 1000 2.25 0.47 2.72 1800 11.93 0.51 12.44 Canadian Mining and Metallurgical Bulletin. April. 1951 2.64 12.72 2.66 12.40 1.47 1.47 0.90 0.90 -- 0.66 -- 0.09 11 12 I 'etc 0 VCfBTYlECAL *0T GAS i EswajST i ; 5\ I'-o-l Flowsheet of a typical asbestos mine ami mill t 13 The Mining, Milling and Grading of Asbestos Fibers In the recovery of Canadian chrysotile, from which most of the asbestos textile products made in the United States are processed, both open pit and underground mining methods are used. Open pit mining is essentially a quarrying operation. Holes are first drilled in the face of the deposit with compressed air drills and the fiber bearing rock is then loosened bv blasting. After a rough separation of ore and barren rock in the pit. the ore is loaded into trucks by power shovels and transported to the mill. Underground mining methods are similar to those employed in the re moval of coal and other minerals. In one method, known as block caving, large blocks of ore are extracted with a minimum of drilling and blasting bv undercutting the ore bodv, then blasting out the supporting columns and allowing the ore to break down from its own weight. The diagrams, page 17. illustrate the progressive steps in mining asbestos bv the block caving method. I -4 5* 5c a An open pit asbestos mine 15 This force jaw crush er is tifpical of those used for primc.rj crushing of the ashestos-bcarinz rock The percentage of fiber recovered from the ore is relatively small, the yield from Canadian mines ranging from three to ten percent depend ing upon the locale and the desired objectives of the operations. This means that from ten to more than thirty* tons of asbestos-bearinO'! rock must be mined in order to produce a single ton of usable fiber, most of which, however, is of insufficient length for spinning. Of the total tonnage of chrysotile asbestos fiber extracted from Canadian mines during 1964, only about two and one-half percent consisted of grades that were suitable for processing into textiles. MILLING Most of the textile fibers produced from the Canadian chrysotile deposits are recovered by mechanical milling and are known as milled fibers. The process is essentially one of freeing the fibers from the mother rock and consists of several stages of crushing, each of which is followed by screen ing and air separation. Although the fibers are tough and strong, specially designed crushing machines and techniques are employed to minimize fiber damage. Enormous jaw crushers, some with a capacity of more than 250 tons of ore per hour, are used for the primary crushing. Secondary crushers. 16 ] :vv.o N QP.C in place / / k'V |V V A >'// x/////,-////. [/.' '////'//. Progressive singes in mining asbestos by the block caving method Shaker screens with suction hoods which lift the asbestos fibers after crushing usually of the gyrating type, effect a further reduction in the size of the ore particles. Other types of crushers and fiberizers are used for addi tional size reduction and opening up of the fibers. Separation is accomplished by passing the mixture of rock fragments and asbestos fibers over large inclined shaking screens. The smaller pieces of rock and the shorter fibers fall through the screen openings and are carried awav for further treatment. As the coarser rock particles and the longer fibers near the end of the screen, thev pass under powerful suc tion hoods. These, functioning like oversized vacuum cleaners, lift the lighter freed fibers but leave the heavier rock particles and the still un opened fibers on the screen. The crushing and screening operations are repeated until all of the fibers bas e been separated and only waste rock remains. After separation, the fibers are further opened, cleaned, graded according to length and bagged in 100 lb. bags for shipment. Although prepared to a considerable extent by the milling process, thev require additional treatment at the textile plant before they are suitable for spinning. 18 COBBING A small percentage of textile fibers (those ranging in length from %" to fi" and longer) are not recovered bv the mechanical milling process de scribed above. Known as crude fibers, these grades are separated by hand cohbinu with a hammer in order to better preserve the long fibers intact. Crude fibers, which are in the form of small unopened bundles, must be fibenzcd at the textile plant. GRADING AND TESTING Since the end uses of asbestos fibers are governed primarily by their length, it is important that they be carefully and accurately graded at the mill. Standard methods of grading chrysotile fibers according to their length have been adopted and generally accepted by the American asbestos industrv. The Quebec Standard Screen Test, used by the Quebec producers, emplovs a machine consisting of three rectangular screens held in frames measuring 24!" by 14i" by 3a" deep, one above the other. The top Operator placing fiber sample in testing machine preparatory to conducting Quebec Standard Screen Test 19 screen is the coarsest, the middle screen is of intermediate si/e and the bottom screen is the finest. Under the bottom screen is a box for col lecting the fibers that pass through all three of the screens. The screens are made to the following specifications: Screen Top-- t Box No. 1) ........................ Middle--(Box No. 2) .................. Boiioin--(Box No. 3) ................ Screen Openinc 0.500" 0.187" < 4-mesh > 0.053" (10-mesh) Diameter of Wire 0.105" 0.063' 0.047" To conduct a test, 16 ounces of fiber are placed on the top screen. The lid is closed and the nest of screens is shaken horizontallv at 327 rpm for 600 res olutions. The fiber grade is then determined on the basis of the number of ounces remaining on each ot the screens and in the collecting box. Thus, if two ounces remain on the top screen, ei^ht ounces on the intermediate screen, four ounces on the bottom screen and two ounces in the box. the fiber is known as 2-S-4-2. one of the spinning grades and is classified as 3T fiber. Other methods of testing are also in use. These include the use of the Bauer-McXett Classifier and the Modified Suter-Webb Comb Sorter. TEXTILE GRADES Canadian Chrysotile: Only the longer, costlier grades of Canadian chrysotile fibers are used in the processing of asbestos textiles. The standard Quebec classifications are as follows: Group Group No. 1 Group No. 2 Group No. 3 'See "Grading" Grade Designation Crude No. 1 Crude No. 2 Spinning Fibers (milled) 3F 3K 3R 3T 3Z Fiber Lencth and longer %" to %~ Guaranteed Minimum Shipping Test1 10.5 3.9 L3 0.3 7.0 7.0 1.5 0.5 4.0 7.0 4.0 1.0 2.0 8.0 4.0 2.0 1.0 9.0 4.0 2.0 20 l*t tiii- Sorter. ia*dian 1s 1. tr g8: j) ^ii t Following are the grade classifications in use at the British Columbia mines: Crude No. 1--basically of crude staple and longer AAA--extra long textile fiber AA--long textile fiber A--textile fiber African Chrvsotile: The Rhodesian milled textile grades are as follows: CS.G/1--a textile fiber equivalent to Canadian 3F C&G/2--a textile fiber equivalent to Canadian 3k C&C 25--a textile fiber equivalent to Canadian 3R CSC, 29--a textile fiber equivalent to Canadian 3T Note: Chrvsotile is also produced as shorter milled fibers, which are suitable for numerous commercial uses but are not of sufficient length for processing into textiles. Crocidolitc: Fully fiberized crocidolite lias a much greater volume than chrvsotile and, to save excessive transportation costs, it is usually sup plied in a semi-milled condition. For this reason it is classified on the basis of length of fiber in the seams or in the unmilled cobs from which the various grades are obtained. Control of quality is normally achieved by comparison with standard or "umpire" samples supplied at regular intervals from the mills. Following are the standard grades of Cape blue (Union of South Africa): Grade S ................................................................... A ................................................................... B ................................................................... C ................................................................... Approx. Lencth Range or Unmilled Fiber Up to w Ms" to %' to 1%' Over I Vi' The following grades of Transvaal blue are as given by the Department of Mines, Union of South Africa.2 Crude TX Tl T2 T3 T4 Fiberized TDX TD1 TD2 TD3 TD4 Lencth or Fiber Plus lVfi" %" to W to %" Vi' to w Minus V4' 2 "Asbestos Crades in South Africa," Asbestos, December, 1948 21 Amosite: For the same reason as stated under "Crocidolite" above, amosite is also supplied in a semi-milled condition and classified on the basis of length of fiber in the seams or unmilled cobs from which the various grades are obtained. Control of qualitv is also achieved by comparison with stand ard or "umpire" samples, supplied at regular intervals from the mills. Fibers from the various mining properties in the Transvaal are graded as shown below: Grade D3 LD3 Dll DX MD M K3 W3 SK SW S2 GK GU S33 Approx. Lencth Rancf. of Lnmilled Fiber 2" to 6" 2" to 6" 1" to 2" 1" to 2" to 2" 9i" to 2" Vi" to 2" Vi" to 2" 3/16" to 1" 3/16" to 1" 3/16" to 1" Vi" to 94" Vi" to 94" Vi" to 94" Designation Long Long (part fiberized) Medium Long Medium Long Medium Medium Medium Short Medium Short Shorts Shorts Shorts Shorts (part fiberized) Shorts tpart fiberized) Shorts (part fiberized) Color Gray Gray Gray Gray Gray Gray Gray Gray Gray Gray Gray Gray Gray Gray aniosite :i <lu' basis of \ '.Mims grades . ,i with stand- ;in- imils. . a;v graded Color ^11 ( j ^ray Cray Crav -rav . rav rav rav rav ''ray Gray Gray Gray Gra\ Gray Flowsheet of a Typical Asbestos Textile Plant BAGGED ASBESTOS FIBER AS REGEIVED FROM MILL CARDED ^ FIBER PREPARATION BLENDING o MIXING s i^arayyp^ >^RAYON. COTTON OR OTHER FIBER FELTING ,:j NON-WOVEN FELTS TAPE CLOTH WOVEN BRAIDED BRAIDED BRAIDED TUBING TUBING CORD ROPE 23 Automatic blending units of the type shown here insure the exact percentages of asbestos and other fibers required for each specific end product Processing Asbestos Textiles Asbestos textiles are produced in modern textile plants by processes which are not unlike those utilized in the manufacture of textiles made from cotton or wool. The successive operations and resultant finished products are shown on page 23 in the flowsheet diagram of a typical asbestos tex tile plant. FIBER PREPARATION The asbestos fibers are received at the textile plant in a fully opened or semi-opened condition. Specially designed opening equipment is used to remove short fibers and to give additional opening when required. The machinery employed for this purpose includes vertical openers, carding willows, box top willows and other devices. 24 i net percentages product BLENDING AND MIXING After fiber preparation, the next step is blending and mixing. The com position of the blends and fixing of the formulation are governed bv the characteristics of the fiber, manufacturing possibilities, the requirements to be met bv the finished product and the intended use. Small percentages of cotton, ravon and other natural or svnthetic fibers are added to improve spinnability and to impart the desired servieeabilitv to the end product. Multi-hopper automatic blending units containing several hopper feeds are employed for the blending and mixing of asbestos and organic fibers. CARDING This operation, similar to that emploved in the processing of wool, com pletes the opening and cleaning of the fibers. Under the teasing action of thousands of needle-pointed wires which form the working face of the "clothing" that covers the cylinders of the carding machine, the fibers are combed into a relatively parallel arrangement, forming a tenuous web. this web. or sliver as it is called, becomes rosing when separated into ribbons, rubbed mechanically and condensed into untwisted strands. Rov ing is the asbestos textile product from which yarns are produced. ocesses which s made from :>.cd products isbestos tex- pcncd or ? is used to ''r'd. The rv ``rding The tenuous web of asbestos fibers from breaker card (foreground) passing over camel back to finishing card SPINNING, TWISTING AND FORMING The previously carded strands of roving are spun into yam in much the same manner as cotton and woolen yams are produced. The spinning pro cess is essentially one of imparting a twist to the roving in order to provide tensile strength and facilitate further processing. The resultant product is known as a single yam. When single yams are twisted together to pro duce larger, stronger yams, the process is known as twisting or plying. Forming is a term applied to twisting single yams into plied yams by means of a tubing twister. A tubing twister feeds two or more single yams of exactly equal length to the spindle, and plies them into a cord having exceptional uniformity and maximum tensile strength. This is done by having the single yams under equal stress so that each contributes its maximum individual tensile to the strength of the cord. The asbestos yams produced by spinning, twisting and forming are made in various sizes and plies and serve as the basic components in the fabrica tion of many other asbestos textile products, both woven and braided. WEAVING Asbestos yam is woven into cloth on looms similar in principle to those used for weaving other types of fabrics. The designated number of strands 26 ) I ourxd) in much the pinning pror to provide .int product thcr to pTOor plying. -d yams bv single yams cord having * done bv ^tributes its J ar' made bdirica:`fJidrd. ' ' `'i'isc ' 'hands I of warp yam are threaded through the heddles and the reed of the loom and sufficient yam is wound on quills and placed in the shuttle for the filling. The warp yams (ends) run longitudinally or parallel to the selvage edges of the fabric, while the filler yams (picks) interweave these together transversely. The construction of the cloth is controlled by regulating the number of ends and picks per inch. Techniques of processing have been developed to such an extent that a large variety of woven products now come from the looms of asbestos textile manufacturers. Fabrics can be woven in flat or tubular shapes and are available in a wide range of textures, weaves, weights and thicknesses. 27 BRAIDING The braiding process is done from a series of yarn-earn ing spindles, half of which travel in one direction and half in the opposite direction. The action is similar to that in a mavpole dance, the yarns being plaited to gether to form a braided product. Many kinds of braids, both round and square, may be produced bv varying the number of ends of yarn wound parallel on the braider tube, by changing the tension applied and by addins mechanical attachments to the braider. FELTING Felting is the process of arranging asbestos fibers or a mixture of asbestos and other fibers to produce a uniform, continuous non-woven sheet. The fibers may have random or parallel orientation. Special binders may be added to provide fabrication strength or other desired properties. INSPECTION AND QUALITY CONTROL During their manufacture, asbestos textiles are carefullv tested for strength, weight, asbestos content and other qualities that are important in the serv ice in which they are to be used. Before packaging, the finished products are given a final inspection to insure that the quality standards established by the manufacturer have been met. 28 pindlcs. half rection. The g plaited to- round and yarn wound lied and bv of asbestos sheet. The iers mav be 1 ties. tested for important e finished standards Asbestos Textile Products Tim: following pages eontain information about the products made from chrvsotile asbestos fibers hv the asbestos textile industry. This includes ? significant test results on strength retention and other properties at ele i vated temperatures. (See "Elevated Temperature Serviceability," page H 31.) Also included is a description of each product and how it is made, together with pertinent data regarding styles, sizes, grades, weights, etc., and a short summary of established uses. Further information, as well as helpful assistance in selecting asbestos textiles for specific applications may be obtained from any of the member companies of the Asbestos Textile Institute. 29 ^ irt 5 -r k * :h-m * 1 n-.ilxn 30 ELEVATED TEMPERATURE SERVICEABILITY \xbestos textiles, used alone or in combination with other materials, find .:,in\- specialized uses, not onlv in the moderate temperature field (up to r . hut also in applications where temperatures in excess of 5000 are encountered for periods of short duration. f'lain 'non-metallic) Asbestos Textiles -- through 900 F: There are two horent factors which have an important bearing upon the serviceability r uiain asbestos textiles at elevated temperatures: 1. The percentage of asbestos in the textile 2. Its design and construction Resistance to degradation by heat is largely a function of the asbestos content: tiie higher the percentage of asbestos fiber, the higher the serv iceability at elevated temperatures. Design and construction, however, Iso influence high temperature serviceabilitv. In general, those textiles v c.ich arc composed of the finer cut yarns will exhibit the highest strength retention characteristics, since these finer varns contain greater amounts cf the long fiber grades of asbestos. Chart A shows the results of 400 to S00' F range tests of strength re tention characteristics made with various grades of plain asbestos fabrics over a 24-hour test period. In interpreting these data, the upper values within each given bar unit should be considered representative of textiles composed of finer cut yams. As the number of yarn cuts decreases, the tensile strength retention will also decrease within the ranges shown. It is also important to remember that the time factor has a direct bearing on the percentage of strength retention. As the elevated temperature period is shortened, the percentage of strength retained is correspondingly increased. This principle is made use of in manv practical applications where asbestos textiles are exposed for shorter periods to temperature ranges greatly in excess of those under discussion here. Conversely, the percentages shown in Chart A represent degradation values approximately S5Cc to 90A of what would be expected in extremely long range sendee over periods of several weeks or months of exposure. Metallic (wire-inserted) Asbestos Textiles -- through 1200 F: These materials, fabricated with an insert of ware, further extend the temperature seniceability range. Their strength retention characteristics are higher than those for plain (non-metallic) asbestos textiles and in addition, they offer greater resistance to abrasion. Laminated and Bonded Asbestos Textiles -- through 5000 F: In the realm of ultra high temperatures, asbestos textiles, combined with resins 31 and ceramic binders, provide a construction possessing a unique combina tion of properties for applications through 5000' F. These properties in clude low thermal conductivitv and diffusivitv, uniform ablation, excellent dimensional stability and high resistance to thermal shock. Particularly outstanding is the low erosion rate of impregnated asbestos textiles at elevated temperatures. As an example, studies indicate an erosion rate at approximately 4000 F for a phenolic resin impregnated asbestos felt of 2 mils per second as compared to S mils per second for boiler plate steel. The low thermal conductivity of these impregnated materials is illustrated in Table L, which presents significant comparative data accumulated bv two different test techniques at temperatures of 4000" and 4500' F. Collumn A shows the results obtained when J" thick samples of the materials under test were exposed to a gas-oxygen flame at 4000= F and the time required to attain a temperature of 360; F on the opposite side of each sample was determined. Column B shows the comparative temperatures on the side away from the flame after a 60 second exposure at 4500: F. The superiority of the felted asbestos laminate as a thermal insulator at these elevated temperatures is clearly apparent. Phenolic Laminated Asbestos Felt Phenolic Laminated Chopped Class Phenolic Laminated Glass Cloth TABLE L A Time Required for Side Away from Flame to Reach 360=F B Temperature Reached O.n Side Away from Flame AriER 60 Sec. Exposure 82 seconds 50 seconds 28 seconds 220F 600 F HOOT 4 I 3 Further evidence of this property is illustrated by a commercial application in which the wall of a solid fuel rocket motor chamber was lined with a Y" thick phenolic resin impregnated asbestos felt. At the 5000 F operat ing temperature, this )' thick insulation protected the wall for the 90 second duration life of the motor, at the same time resisting the destruc tive erosive action of the high velocity exhaust gases. Recent developments have added a new group of ceramic bonded asbestos textiles for ultra high temperature service. These new materials are formu lated and fabricated by impregnating asbestos textiles with specially com pounded ceramic metallic oxides and silicates. The resulting products are 32 i nique eombina properties in'ation. excellent .k. Particularly stos textiles at r. erosion rate d asbestos felt der plate steel. Is is illustrated .cumulated bv 4500- F. Col1 the materials and the time - side of each temperatures e at 4500' F. insulator at - Reached On erom Flame >c. Exposure :0F >0oF iVF d application lined with a '0C F operat1 for the 90 the destruc- h'd asbestos ;>re formu- > illy comr,"hicts are I niueable at temperatures above 3000 F and are lighter in weight and iii withstand more physical abuse than conventional ceramic products. iTv exceptionally good resistance of asbestos to nuclear radiation india;. > that this fiber, either in textile form or as a reinforcing agent in an rnropriate matrix, will have important applications in environments uxnnseu to such radiation. .uuies have shown that asbestos fibers can withstand an integrated epihicnnai neutron flux of approximately 1020 NAT before significant struc- Thc word "grade" as used in the asbestos textile industry indi cates a system of classification based on the percentage of asbestos by weight in the finished product. In Table K are listed the standard grades with the percentage of asbestos content for each grade.1 This method of grading applies to all products described on the following pages except carded asbestos fibers, although not everv product is manufactured in vverv grade. The available grades will be found listed under each product TABLE K PERCENTAGE OF ASBESTOS CONTENT BY WEIGHT IN ASBESTOS TEXTILE PRODUCTS As Established by the American Society for Testing and Materials Grade Commercial ........................................ l mlerwriters' .................................... Grade A .............................................. ('rade A A .......................................... Grade AAA '........................................ Grade AAAA .................................... Asbestos Content by Weight 75% up to but not including 80% 80% up to but not including 85% 85% up to but not including 90% 90% up to but not including 95% 95% up to but not including 99% 99% up to and including 1(X)% 'See A>TM Specification D 1918. page 92. for the test methods used to determine asbestos content (grades). 33 Asbestos Lap Asbestos lap is a felted form of carded asbestos fibers which have been blended with organic fibers. It is furnished in two stvlcs: Stvle I, a single ribbon-like formation of fibers, and Stvle II, a paralleled assemblage of Style I lap. Uses: A specialized product made for the electric wire and cable industrv, asbestos lap is designed for re-carding into an insulation for heater cords, fixture wires and other electrical conductors. The re tarded laps arc spiraled around the conductor to form a homogeneous wall of asbestos 34 ive been a single blagc of hidustrv, ' r cords, -'! arc 'bestos i .rs which sen e as a carrier for the electrical insulating compounds. The - miovment of asbestos to completely envelop certain tvpes of copper ; es w hich mav be exposed to severe heat has long been a requirement .National Electrical Code in the interest of preventing electrical fires. . ,-.:ues. Weights: Asbestos lap is made in the following standard ASTM s: L'nderwriters', A, AA and AAA. (See Table K, page 33. for per- :ir,,_:e nt asbestos content in each grade.) It is supplied in unit rolls * i'J-!ii trom 250 to 4200 grains- per linear yard.*3 4 Icctrical Insulation Classification: Asbestos lap as made for the elec,:i indnstrv is furnished in three types, classified on the basis of mag- '.)c rating determinations'* which serve to identify performance limits. Tvpe II -- Magnetic Rating 0.75 Maximum Tvpe IV-- Magnetic Rating 2.00 Maximum Tvpe VI --Magnetic Rating 4.00 Maximum Tvpe II is intended only for special applications where the asbestos is of vnmarv importance as electrical insulation used on magnet wire and when used primarily as a dielectric. Type IV is intended for use where the asbestos is of secondary importance as electrical insulation and where it is applied in combination with other materials of comparably higher dielectric strength, as in the construction of heat and flame resistant electrical insulating walls over unit conductors of electric cables. Type VI is intended for use where the asbestos is of minor importance as a dielectric, as in the construction of filler or heat and flame resistant walls of electric cables or when used as a lining for control enclosures subject to exposure to electric arcs. Standard Packages: Asbestos lap, wound on paper tubes, is packaged in rolls which vary in size in accordance with the number of slivers in the assemblage. -Grain: a unit of weight. 7000 grains = 1 pound. 3For permissible weight variations, methods of test and other detailed information about asbestos lap not given above, see ASTM Specification D 1001, reproduced on paces 60 and 61 of this Handbook. 4See ASTM Specifications D 2100, page 78, and D 1118, page 81. 35 Asbestos Roving Asbestos roving is an assemblage of carded asbestos fibers blended with cotton or other organic fibers and condensed into a single strand without twist. It is produced in various degrees of density from a soft, fluffy roving to a firmly compacted one, to meet specific requirements of the user. Reinforced roving (also known as core or inserted roving) is similar to the plain roving described above but has a core of cotton or other thread to give it added tensile strength. Uses: Asbestos rovings were developed for the electric wire industry to serve as insulation for heater cords, cables and electrical heating elements and are extensively used for this purpose. The strands are wrapped or "served" by wire covering machines to form a relatively soft, complete sleeye over the wire. Grades: Asbestos roving is supplied in five standard ASTM grades: Underwriters', A, AA, AAA and AAAA. (See Table K, page 33, for per centage of asbestos content in each grade.) Size or Cut: The size of asbestos roving is denoted bv the "cut" number which, when multiplied bv 100 indicates the approximate number of >lended with and without Huffy roving the user. is similar to other thread industry to g elements " rapped or 't. complete 'M grades: '}> for per- '"inihcr "aoln-r ,,f i i cis per pound. Standard cut numbers, with nominal yards per pound ..id nermissible variations are shown in Table 1, ASTM Specification ' .'75 reproduced on page 63. lectrical Insulation Classification: Asbestos roving as made for the vtrical industry is furnished in three tvpes, classified on the basis of . -.nguetic rating determinations5 as follows: 7 ee II (Magnetic Rating 0.75 Maximum) is intended only for special indications where the asbestos is of primary importance as electrical in.ui.uion used on magnet wire and when used primarily as a dielectric. ' pe iV (Magnetic Rating 2.00 Maximum) is intended for use where he asbestos is of secondary importance as electrical insulation and where h is applied in combination with other materials of comparably higher dielectric strength, as in the construction of heat and flame resistant elec trical insulating walls over unit conductors of electric cables. Tvpe VI (Magnetic Rating 4.00 Maximum) is intended for use where the asbestos is of minor importance as a dielectric, as in the construction of filler or heat and flame resistant walls of electric cables or when used as a lining for control enclosures subject to exposure to electric arcs. Standard Packages: Asbestos roving is wound on cones and tubes of various sizes in accordance with customer requirements. 5See ASTM Specifications D 2100, page 78, and D 1118, page 81. 37 tensile os tex' such. elecristics e, ase are fiber synuringO plain nore e of x as > ted "t - 1 5 1 | 1 * i si I -v Metallic varns are widelv used in asbestos textiles where the :.i ouuct rccjuires unusually high tensile strength, exceptional re duce to heat or abrasion, or a combination of these properties. ! iss C: Organic Reinforced Asbestos Yam is plain asbestos yarn with an r. : t varn made of other fibers, usuallv cotton and or one of several ;.:ctic organic fibers. Reinforced varns, also referred to as inserted ms. arc particularlv adapted to the braiding and weaving processes . c:sc of their increased tensile strength. '.lvs D: Inorganic Reinforced Asbestos Yarn is plain asbestos yam connnn-metallic reinforcing strands such as glass fiber yams. d.;ss E: Combination Yarns are asbestos yams constructed of two or ore of the varns described in Classes A through D, or yarns containing forcing members from two or more of Classes A through D. ''r^ic and Plied Yams: Asbestos yarns are produced as both single and e(i varns. Plied varns consist of a number of strands of single yams vied together to form a heavier yarn of greater strength. Treated Yarn: For special purposes, asbestos yarns are also coated or im pregnated with various compounds to lay the fibers or increase tensile strength or impart other properties. These are known as treated yams. Grades: Asbestos yarns are made in all standard ASTM grades as follows: Commercial, Underwriters', A, AA, AAA and AAAA. (See Table K, page 33, for percentage of asbestos content in each grade.) Direction of Twist: Asbestos yarns are spun with "S" and "Z" twists. (See Glossary, page 99.) Cut of Yarn: The term "cut" refers to the number of 100 yard lengths contained in a pound. (See also "Cut, Asbestos" in Glossary, page 97.) Yarn Numbers: In the asbestos textile industry, the yam numbering system used designates the cut, number of plies, and whether the yarn is plain or contains a metallic insert. In a four digit figure, the first two digits indicate the cut, the next digit indicates the number of plies and the final digit indicates the number of metallic strands. If the final digit is a zero, it indicates a plain (non-metallic) yam. For example. No. 2430 is a 24-cut, 3-ply plain yam. No. 1022 is a 10-cut, 2-ply metallic yam containing two wires as the metallic inserts. In a three digit figure, the first digit indicates the cut. Thus, No. 810 is an 8-cut single ply plain yam. Standard Packages: Asbestos yarns are wound on paper tubes or cones. Various size packages are available to meet the user's requirements. 39 Asbestos Cord Twisted asbestos cord is made of a predetermined number of strands of asbestos yarn tightly twisted together to form a cord of specified diameter and higher tensile strength. The yam used may be single or plied, sized or unsized, or plain (non-metallic) or metallic (wire-inserted), depending on the end use of the product. Braided asbestos cord is made by braiding one or more jackets over an asbestos yam or cord core. Uses: Because of their uniformity', strength and ability to withstand high temperatures with negligible structural change, asbestos cords have many specialized uses. They provide an ideal core for electric resistance wires and are widely employed as an insulation for glass handling tools, as a seal on high temperature corrugated metal gaskets, as a valve stem pack ing and as a braided wall in the construction of steam hose. The metallic cords have inserts of fine wire and are designed for use under exceptionally severe conditions. They are especially suitable for flare signal cords and for such uses as suspending retorts, crucibles and other objects that are in contact with flame or heat. 40 V.uics: Asbestos cord is made in all standard ASTM grades as follows: .'ommercial, Underwriters', A, AA, AAA and AAAA. (See Table K, page 33, -'T percentage of asbestos content in each grade.) :zcs: Standard diameters of asbestos cord range from Via" up to ''reetion Of Twist: Asbestos cords are plied with "S" and "Z" twists. ,'e Glossary, page 99.) lannard Packages: The form of package varies with the requirements of e customer. Fractions of a pound are usually packaged as balls; quan gos of 1, 5 and 10 pounds are generally wound on tubes or spools; rgcr quantities up to 50 pounds are on spools or reels. TABLE M--WEIGHTS AND FOOTAGES OF ASBESTOS CORD Nominal Diameter Inches Approx. Lbs. Per 100 Ft. Approx. Ft. Per Lb. 1/16 3/32 1/8 5/32 3/16 1/4 .20 .40 .63 .95 1.43 2.00 500 250 160 105 70 50 Asbestos Thread Asbestos thread is made by treating asbestos yarns with special com pounds to lay the fibers and to produce an exceptionally smooth, uniform finish. It is produced in both plain (non-metalhc) and metallic (wire-in serted) classes, the latter being noted for its great tensile strength and high thermal stability. It is adapted to either hand or machine sewing. Uses: Because it possesses the advantages that are inherent in the inor ganic mineral fibers from which it is made, asbestos thread can be used under conditions that would be destructive to thread made from organic fibers. Typical uses include sewing the asbestos fabrics used in the manu facture of theater curtains, belting and safety clothing; sewing insulation jackets on piping and turbines; wrapping electric resistance wires; and fastening the asbestos roving insulations at each end of heater cords. Grades: Asbestos thread is generally furnished in Underwriters' grade. Standard Packages: Asbestos thread is supplied wound on tubes as speci fied by the user. 41 Asbestos Cloth Asbestos cloth is woven from five classes of asbestos yarns. The most wiilelv used fabrics are woven from Class A (plain or non-metallic) yams and Class B (metallic or wire-inserted) yams. Other fabrics are made from Class C, D and E reinforced yams as described in ASTM Specification D 1571, pace 70. A wide selection of grades, weights and constructions is available and textures range from open-mesh to lightproof. The choice of weaves includes plain, twill, broken twill, satins and herringbones. Representative fabrics are shown on the following pages. In addition to the standard asbestos cloths, specially treated cloths are made bv most asbestos textile manufacturers to meet unusual conditions or tq prov ide special characteristics such as resistance to extreme abrasion. APPLICATIONS Because of its inherent incombustibilitv and thermal stability, asbestos cloth is extensivelv used wherever these properties are essential in a fabric. Familiar examples are the asbestos safety curtains of dieaters and auditoriums, flameproof draperies, fire-smothering blankets, and the safety clothing worn by members of the armed services and by industrial workers as protection from intense heat and flash burns. Asbestos cloths with suitable treatments or coatings are widely used as the facings for conveyor belts handling hot materials; as covers for domestic ironing boards and commercial laundry flat work ironers; as gasketing material for high temperature and pressure boilers and pipe flanges; and as industrial furnace hoods, shields for welding booths and splash aprons. Many government specifications, particularly those of the United States Navy, require that high pressure steam pipe insulation be protected by an outside jacket of asbestos cloth. Maritime specifications, and many in dustrial and utility power plants also require asbestos cloth to protect the insulation and to serve as a fireproof jacket over pipe and boiler insulation. Underground and overhead piping, both steam and refrigera tion, as well as heating and ventilating ducts, are best protected by a jacket of asbestos cloth. Specially processed lint-free asbestos cloths also serve as protective shields in "clean" areas adjacent to nuclear reactors. The dust bags for removing dust, fumes and vapors in mechanical dust collecting systems are among other specialized uses of asbestos cloths. In the glass industry they serve as lehr curtains and to prevent contact be tween molten glass and cold metallic surfaces. In the field of sound 42 -ns. The most aetallic) yams ire made from Specification constructions t. The choice herringbones. "d cloths are al conditions me abrasion. litv, asbestos scntial in a heaters and id the safety v industrial lelv used as covers for ironers, as rs and pipe booths and nited States rotected by id many in to protect and boiler d refrigeraeeted by a cloths also ir reactors. mical dust ' eloths. In "ntact be- of sound i 'i. >;vciallv fabricated asbestos cloths proxide acoustical properties ;.ii are utilized in reducing undesirable noise levels. ' vatcd Asbestos Cloth: To meet the special requirements ol the plastics iestrv. asbestos cloths, impregnated with organic resins and press cured. :.ie .>bestos-base plastic parts lux-ins lush impact resistance and I .... at iiexural and tensile properties. The most comimmlv used resins i niienolics. silicones, melamines and acrvlics. ; r'eket and missile industries utilize resinated asbestos components | thev provide a lush strength to weight ratio and also a uniform .a rreciictable rate of ablation. Several tvpes of asbestos brake linings .0 clutch facings are made from asbestos cloth impregnated with eatable compounds. '.. audition to the organic tvpe resins, inorganic compounds are also inbined with asbestos cloth to provide hi till thermal insulatin'! value, :s::t weight and exceptional resistance to phvsical abuse. j Metallic ixx ire-inserted) Asbestos Cloths are noted for their superior | tensile strength and high resistance to heat and abrasion. These (|ualities stake them virtually indispensable as a base in automotive and industrial friction materials, mechanical packings and gaskets, aircraft firewall and aerodynamic seals, and as jacketing oxer insulation on high temperature steam generators and turbines. Aluminized Asbestos Cloth: By bonding an aluminum foil or film to a selected asbestos cloth, the properties of superior strength retention under prolonged heat exposure, high thermal reflectivity, and high re sistance to frictional wear are obtained. As safety clothing and as blankets, hoods, curtains, etc., aluminized asbestos cloth forms an effec tive protective shield which reflects 90^ of radiant heat and harmful infrared rays. The mirror bright aluminum surface, which is both attractive and durable, also adapts to such diversified uses as a maintenance-free insulation jacket for steam pipes, a flameproof wall and ceiling covering, and as a flexible air conductor for heating, cooling and ventilating equipment. Asbestos Dryer Felts: This product is another example of the adaptability of asbestos textiles to an industry's specialized problems. Formerly, the dryer felts used on papermaking machines were generally made of all wool or all cotton yarns. These felts, under the deteriorating effect of [ heat, moisture and acidity, required frequent replacement. In the asbestos dryer felt, asbestos yams are combined with cotton and certain synthetic yams in such a way that the fabric is protected with a complete and un- 43 `- V V* Jvi ww V *1 * / J j-j i v'.WA'A - 1J > i U 4^ ' . M umm Wms ATTf Style* Nofcr 40P1 ov 44 .surface of asbestos. Now used in many of the paper mills of the "aired States and Canada, this improved felt is giving from two to Eve .vs the serviceability of the ordinary felt, thereby effecting large savings :i replacement costs. It also assures faster, more even drving with better ' :idi and increased production rates. irades: Asbestos cloth is made in all standard ASTM grades as follows: mmercial. Underwriters, A, AA, AAA and AAAA. In general, the /varies containing the higher percentages of asbestos provide greater ermai stability. (See Table K. page 33, for percentage of asbestos eonnt in each grade, and Chart A. page 30. for strength retention properties). Widths: Asbestos cloth is generally available in widths of 36". 40" and 60". :;dier widths are woven for special applications. Weights: The style designation employed bv the ATI uses both a numeri cal and alphabetical classification. In metallic cloths, the first two digits denote the weight per square yard expressed in ounces. The letter "M" indicates that the fabric is made with metallic or wire-inserted yams, and the final digit or digits indicate the cut number of the yarns employed. In plain or non-mctallic cloths, the meaning of each numerical designation ATI* Stylet Nov 19H-1201 is the same as that used in the metallic cloth classification. The alphabeti cal letter designates the weave used. The letter "P" stands for plain weave, "H" indicates a herringbone construction, and "T" denotes a twill. Tables X and P give weights and constructions of t\-pieal asbestos cloths. Thicknesses: The thicknesses of single plv cloths range from approximately .015" to .100". Fabrics up to 15" in thickness can be woven in multi-ply construction. Tolerances: The tolerances for width, weight, thickness, yarn number ;Clit) and construction of asbestos cloth are in accordance with ASTM Specification D 1571. See page 71. Standard Packages: Asbestos cloth is normallv supplied in rolls of 50 and 100 linear cards. Other lengths can be ordered. table x-coxstri ctiox of typical metallic i W1RE-1XSERTED > ASBESTOS CLOTHS W i ibiil Lt. v 11> 2.00 2.00 2.15 2.25 2.30 2.44 2.50 2.50 2.50 2.75 2.75 2.75 2.75 2.80 2.90 3.00 3.00 3.25 3.45 3.45 3.50 4.00 4.25 6.25 7.00 ATI NTYLE No. 32M8 32.M12 35M10 36M10 37.M12 39M10 4OM10 40M10 40.M12 44.M8 44M9 44M10 44M10 45.M12 46M10 48M8 48M10 52M10 55M8 55M10 56.M10 64M10 68M10 100.M12 112M10 Constriction i Ends | Picks tVsRP | Ttu. Yarn I Yarn 14 14 19 9 18 8 18 8 18 8 18 9 17 8 12 7.5 18 8 14 10 17 8 18 9 14 8 18 9 19 10 16 10 18 9 20 10 16 7 18 9 18 9 22 10 16 8 45 15 35 12.5 811 ) 811 1221 | 1211 1021 i 1011 1021 1 1221 ! 1011 1221 1021 1021 1021 1021 1022 1022 1021 1221 822 821 921 921 1021 1021 1022 1022 1021 1221 1021 1021 822 821 1022 1021 1021 1021 822 822 1022 1022 1022 1022 1022 1022 1032 1032 1221 1221 1022 1022 The Lrtlcr "M" ill Suit- Number indicates Metallic Cloth. 46 TABLE P--WEIGHT AND CONSTRUCTION OF TYPICAL PLAIN (NON-METALLIC) ASBESTOS CLOTHS Weight Lr.s, ^ d ~ (( ATI Style No. o.r.o 0.65 0.70 0.75 0.50 0.95 1.05 1.05 1.10 1.20 1.25 1.30 1.30 1.40 1,10 1.40 1.45 1.50 1.65 1.65 1.65 1.75 1.80 1.80 1.95 2.00 2.10 2.25 2.25 2.27 2.35 2.50 2.50 3.00 3.00 3.30 3.70 4.20 4.75 5.25 -5.50 8P26 1CP24 11P20 12P13 14P17 15P26 17P10 17P24 1SP10C 191120 20P28 21P10 21P16 221'10C 22P16 1 O p 11 23P18 21P10 26P10 26P12 26P14 28P16 29P10 29P14 31P12 32P12 34P10 36P8 36P10 37P10 38P12 40P10 40H14 48P10 48T12 53T12 59T12 67P10DC 76P10DC 84P10DC 88P10DC Ends CONSTRUCTION Picks \\ ARP Yarn Fill Yarn 20 14 21 22 21 17 21 17 21 19 15 14 2u 15 16 15 13 9 35 27 27 13 88 12 15 18 9 19 10 21 12 17 14 99 10 10 13 13 14 14 24 10 16 10 20 10 10 11 18 9 16 9 16 6 18 9 18 10 20 12 20 10 28 14 18 9 30 10 36 12 40 14 30 14 37 16 40 15 40 13.5 2610 2110 2010 1810 1710 2620 1010 2120 1010 2010 2820 1020 1620 1010 1620 2220 1820 1020 1020 1220 1420 1620 1020 1420 1020 1220 1020 820 1020 1020 1220 1020 1420 1030 1220 1220 1220 1020 1020 1020 1020 2610 2410 2010 1810 1710 2620 1710 2420 1010 2010 2820 1020 1620 1010 1620 2220 1820 1020 1020 1220 1420 1620 1010 1420 1230 1220 1020 820 1020 1120 1220 1020 1420 1020 1220 1220 1220 1020 1020 820 1030 Tensile Strength* Warp Fill 30 25 40 45 40 30 40 30 55 50 45 40 65 40 55 50 90 70 100 75 80 40 45 40 55 70 11!o 70 80 40 To 35 55 50 50 45 55 50 65 60 75 70 115 50 90 30 95 40 55 100 90 40 90 45 100 40 125 50 135 55 105 55 135 55 160 70 180 55 170 50 180 55 -- -- ---- ---- -- -- ~~ The letter "P" in Style Number indicates Plain Cloth. "H" indicates Herringbone Construction. "T" indicates Twill. * Minimum average of 5 tests, grab method, according to ASTM Specification D 1682. 47 Asbestos Tape Asbestos tape is a narrow woven fabric with selvage edges. It is made in five classes, the most commonly used being Class A, a plain or nonmetallic tape, and Class B. a metallic or wire-inserted tape. The other three classes are described in ASTM Specification D 315, page 74. Uses: Asbestos tapes are widely used in the electrical industry as an insula tion and have numerous other applications where an incombustible woven tape of high tensile strength and thermal stability is required. Plain (non-metallic) Tapes of thin dimension are designed primarily for electrical insulating purposes such as motor w indings, where there is need for a heat conductive, thermally stable insulation capable of absorbing a high percentage of insulating varnishes and treatments. The impregnated tape forms a moisture barrier essential to efficient motor operation. Heavier plain tapes are w idely used as a durable flameproof wrapping for lead sheathed cables, as an insulation for pipe hangers, as safety protection for covering hot piping, as stress-relieving pads in welding operations, and as a component of packings and gaskets. When specially treated, these tapes provide such advantages as arc proofing and resistance to oil. water and corrosion for electrical cables; they can also be produced to withstand the destructive action of thermo-mechanical forces for other applications. 48 --'s. It is made plain or nonThe other 74. ' as an insulamxtible woven d. primarily for du>re is need -'hsorbincr a 'mpregnated Jt ion. "rapping for Protection and Hu-se ' ,:i1 " tter "V'! A*id 1 * >'Ills. Metallic (wire-inserted) Tapes are designed for service requiring higher tensile strength or a high coefficient of friction or where extreme abrasive eonditions are present. They are used as the major component in woven brake linings and clutch facings and as oil burner wicking. These tapes re woven with special allov wires for applications where excessively high `jmDeratures are encountered. The thermal stabilitv of asbestos tape adapts it particularly for use as a convexor belting for earn ing hot materials. Both plain and'metallic tapes are made for this purpose. Some are woven with the top plv of plain earn and the bottom plv of metallic varn to resist stretch and may be specially treated to increase resistance to abrasion. Grades: Asbestos tapes for electrical purposes are made in Underwriters' grade. Tapes for other uses are available in all standard ASTM grades from Commercial through AAAA. In general, the tapes with higher as bestos content are used where high temperature conditions are encoun tered. (See Table K, page 33, for percentage of asbestos content in each grade.) Thicknesses, Widths: Standard thicknesses of thinner plain tapes range from .010" up to .030". Greater thicknesses can also be furnished. Heavier plain tapes are made in thicknesses up to Metallic tapes are woven in thicknesses of ] and heavier. Standard w idths of asbestos tape range from ]>" to 6". Tolerances conform to ASTM specifications.0 Weights: The weight of asbestos tape varies from fractions of a pound to more than 100 pounds per 100 feet, depending on size. Tables Q and R show the approximate number of pounds per 100 feet and the approxi mate footages per pound of tapes of standard thicknesses and widths. Tapes of weights other than those shown can also be woven. Electrical Insulation Classification: Asbestos tape as made for the elec trical industry is furnished in three types, classified on the basis of mag netic rating determinations*7 which serve to identify performance limits. Type II (Magnetic Rating 0.75 Maximum) is intended only for special applications where the asbestos is of primary importance as electrical in sulation used on magnet wire and when used primurilv as a dielectric. c For permissible variations in thickness, width, weight and construction, and other data about asbestos tape not given above, see ASTM Specification D 315, page 74. 7 See ASTM Specifications D2100, page 78, and D 1118, page 81. 49 Tvpe IV (Magnetic Rating 2.00 Maximum) is intended for use where the asbestos is of secondary importance as electrical insulation and where it is applied in combination with other materials of comparably higher dielectric strength, as in the construction of heat and flame resistant elec trical insulatina walls oxer unit conductors of electric cables. Tvpe VI (Magnetic Rating 4.00 Maximum) is intended for use where the asbestos is of minor importance as a dielectric, as in the construction of filler or heat and flame resistant walls of electric cables or when used as a limner for control enclosures subject to exposure to electric arcs. Standard Packages: Asbestos tapes for electrical insulation (plain tapes up to and including .030" thick) are generally furnished in 36 yard rolls wound on bushings. Industrial tapes of *32" and greater thickness are furnished in 100 and 150 foot rolls. TABLE Q--METALLIC i WIRE-INSERTEDi WOVEN ASBESTOS TAPE Asbestos Textile Institute Standards" Thickness Width Anrnox. Fr. Approx.Lbs. Inches 1 scuts Per Lb. Per 100 Ft. Thickness Width Approx. Ft. Approx.Lbs. Inches Inches Per Lb. Per 100 Ft. 1/16 v. r* i 1 Vi l>i 2 2 Vi 3 3 Vi 4 4 Vi 5 5 Vi 6 Vs % i 1V4 l'/j 2 2 Vi 64.1 42.7 32.0 23.9 19.0 15.1 12.1 10.0 &61 7.53 6.71 6.04 5.49 5.03 16.9 127 10.9 9.6 6.6 5.6 1.56 2.34 3.12 4.18 5.25 6.62 8.26 9.93 11.61 13.24 14.90 16.55 18.21 19.87 5.9 7:9 9.1 10.4 15.2 17.9 Vs bl/2 6 3 3 Vi 4 4 Vi 5 Vi i 1V4 lVi 2 2Vi 3 3Vi 4 4Vi 5 SVi 6 2.5 39.9 2.3 43.4 4.4 22.6 3.8 26.1 3.4 29.5 3.0 33.0 2.7 36.4 7.1 14.1 5.7 17.6 4.7 21.2 3.5 28.3 2.8 35.4 2.3 43.6 2.0 50.0 1.8 56.3 1.6 62.6 1.4 70.4 1.3 77.4 1.1 83.7 8 Tapes can also be supplied in greater widths and thicknesses. 50 lse where md where >lv higher tant elee- se where istruetion n used as iin tapes ard rolls mess are '5 TAPE PPROX.LbS. i n 100 Ft. 39.9 13.4 -'2.6 -'6.1 -'9.5 3.0 '6.4 1.1 :.6 1.2 3.3 >.4 .6 .0 .3 .6 l 1 TAULE R--PLAIN' (XO.VMETALLIC) WOVEN ASDESTOS TAPE Asbestos Textile Institute Standards1' !':mi K'k- - W idth Approx. Ft. AprRox.Lcs. Thickness W idth Approx. Ft Approx.Lbs. 1 \tlli_S 1'iR Lb. I'm 100 Ft. Inches Inches I'er Lb. I'er 100 Ft. , .'10 1 1A !'- 1A .015 .020 .0J5 .030 1/32 i i'. i:j I *> i i Hi i'j 1AO i . r 1 Hi 1'. ia 2 2>:. 3 1/, A 1 111 1*5 IA 2 2'.i 3 V* 1 Hi 120.0 291.0 222.0 183.0 155.4 133.8 117.3 276.0 198.9 153.6 126.0 103.0 99.0 84.0 224.4 159.9 123.3 100.5 84.9 73.5 64.8 168.9 119.4 92.4 75.0 63.0 54.9 48.6 37 6 31.5 134.1 90.9 68.7 56.4 47.7 40.8 36.0 28.2 23.8 125.0 84.7 60.2 50.0 0.24 0.3 4 0.45 0.55 0.6 4 0.75 0.85 0.36 0.50 0.65 0.79 0.93 1.00 1.18 0.45 0.03 0.81 0.99 1.18 1.36 1.54 0.59 0.84 1.08 1.33 1.58 1.82 2.06 2.66 3.16 0.75 1.10 1.46 1.77 2.10 2.45 2.78 3.54 4.20 .80 1.18 1.66 2.00 L-32 1/16 1/16 Hi 2 ?i 3 l ; `.`4 i i]i 1U- 0 oi 3 3'i 4 4i;- 5'A 6 Vs 7* 1 Hi 11 Vi 2 2 Vi 3 3Vi 4 4Vi 5 5Vi 6 %1 1% Hi 2 2 Vi 3 3 Vi 4 4Vi 5 5Vi 6 41.7 32.2 26.3 22.2 81.3 50.0 40.5 31.5 26.3 19.4 15.2 13.2 11.2 9.9 8.8 7.9 7.1 6.6 21.3 15.9 13.6 12.0 8.2 7.0 5.5 4.8 4.2 3.8 3.4 3.1 2.9 8.3 6.7 5.6 4.2 3.3 2.8 2.4 2.1 1.9 1.7 1.5 1.4 2.40 3.10 3.80 4.50 1.23 2.00 2.47 3.17 3.80 5.16 6.60 7.60 8.9 10.1 11.3 12.7 14.0 15.2 4.7 6.3 7.3 8.3 12.2 14.3 18.1 20.8 23.6 26.4 29.1 32.0 34.8 12.0 15.0 18.0 24.0 30.0 36.0 42.0 48.0 54.0 60.0 66.0 72.0 * Tapes can also be supplied in greater widths and thicknesses. 51 Asbestos Tubing Asiu:.stos tubing. sometimes calk'd tubular sleeving. is made from asbestos varus, cither braided or woven. The braided stvle is supplied in mam' diameters ami textures and in several wall thicknesses to meet a varietv of service conditions. It is furnished untreated or treated, as mav be re quired. The woven style can he manufactured in various constructions and is usnnllv made to specification. Uses: Braided asbestos tubings arc widely used as a sleeving for electrical appliance leads, cables and other conductors to pros ide fire protection and resistance to mechanical abrasion. Thev are also extensively used for covering the lead w ires of thermocouples and in the glass industry thev protect the hot glassware from injury by serving as a covering for pincers and tongs. An important practical advantage of braided tubing is the ease with which .it can be fitted over the surface to he covered. A braided tubing will slide readilv over a rod. wire or cable of the same outside diameter as the inside diameter of the tubing, and if necessary its flexibilitv will allow it to be expanded or contracted to fit slightly larger or smaller diameters. 52 ".oven stele of asbestos tnl>in<i is particularlv adapted tor the insnlaMi ot bus liars. Woven tubing of large diameters is sometimes formed uo the dust bags used in pneumatic svstems for filtering hot waste gases li constitute a fire and dust hazard.' : .i .k'r'm Asbestos tubing is made in all standard ASTM grades -- Com:t. Underwriters'. A. AA, AAA arid AAAA. (See Table K. page 33. r Percentage ot asbestos content in each grade. ) | 'izes: braided tubings are produced w ith inside diameters ranging from 1 im ro several inches. W all thicknesses range from less than ,:;j" to ..;ipro\:matelv 1 s". W oven tubings are made in diameters from less than 1" up to 22K". Mandard Packages: Braided tubing is packaged on spools in quantities ranging trom 5 lbs. for thin walled tubing to 50 lbs. for heavv walled : doing. Woven tubing is sold in rolls, or cut to specified lengths. i'll asbcWo.! in mam ; a varietv uav lie ru ctions and electrical protection used tor >'trv thee >1 JlilKtTS " l.idi ""'I will '*r! the I s See also "Asbestos Cloth," page 42. 53 Asbestos Wick Asbestos wick is a soft pliable strand of asbestos formed by looselv twist ing together several strands of roving, stubbing or felted asbestos. It is supplied either with or without cotton varn reinforcement. Uses: Furnished in convenient ready-to-use form, asbestos wick is a gen eral utility product of many and varied applications. The power plant engineer keeps it liandv as an emergency packing. The plumber finds it useful for packing steam and hot water valves. The roofer depends on it as a weather seal for corrugated roofing. Maintenance workers use it for caulking retorts, for sealing ovens and furnace doors and similar jobs. Specially designed asbestos wick is used to wipe excess metal from wire in the process of tinning and galvanizing and as a core for high tempera ture packings. Grades: The standard grade of asbestos wick is Commercial but other grades are supplied on order by most manufacturers. (See Table K, page 33, for percentage of asbestos content in each grade.) Sizes: The l/4 " diameter is standard for most purposes but other diameters (usually from 'i" or up to or Vi") are also furnished. Standard Packages: Asbestos wick is sold in liandv ]/4, % and 1 pound halls and in larger quantities (usually 10, 25 and 50 pounds) wound on spools or reels. 54 Asbestos Rope This product is produced in two styles: twisted and braided. Twisted asbestos rope is made by twisting tightly together two or more strands of asbestos wick. In the heavier ropes, a binder is generally used to hold the twist. Braided asbestos rope is made in three constructions: (1) by braiding one or more jackets of asbestos yarn over a core of asbestos rope or wick; (2) by braiding asbestos yarn braid over braid to form a finished product of either square or round cross-section; and (3) by plaiting asbestos yarn into square cross-section. The braid over braid rope is firmer and stronger; the plaited rope is softer and conforms more readily when compressed. Uses: Asbestos rope, a companion product to asbestos wick, is used where a thicker material than wick is desired. The twisted style is widely used as a seal between furnace doors and brickwork, as a filling for expansion joints in plastic walls of boiler settings, for covering diesel engine exhaust lines, for packing boiler expansion and gas generator doors, as a gasketing material for manhole covers and as a core for high temperature packing. The braided style is used as a groove packing for inspection doors, as 55 Ellin" for expansion joints in furnace brickwork, as a gasket for sealing doors of water gas generators and similar services. Crades: Asbestos rope is furnished in Commercial grade for most general uses and in Underwriters', AA. AAA and AAAA grades to meet particular service requirements. The grades with higher asbestos content are used for high temperature applications. (See Table K, page 33, for percentage of asbestos content in each grade.) Sizes: Asbestos rope is made in a wide range of diameters, usually from '4" up to l' .j" or 2". Standard Packages: Asbestos rope is generally sold in 10, 25 and 50 pound units wound in coils or on reels and packed in individual cartons. TABLE S--APPROXIMATE WEIGHTS AND FOOTAGES OF ASBESTOS ROPE Nominal Diameter Inches % % '!H % % 1 1% Ifc Approx. Lbs. per 100 Ft. 2.5 5.0 8.5 12.5 16.5 25.0 31.0 40.0 56.0 Approx. Ft. per Lb. 42.00 20.00 11.75 8.00 6.10 4.00 3.00 2.50 1.80 56 a gasket for sealing ule for most general -s to meet particular ns content are used e 33. for percentage meters, usuallv from in 10. 25 and 50 individual cartons. rOOTAGES pprox. Ft. per Lb. 42.00 20.00 11.75 8.00 6.10 4.00 3.00 2.SO 1.80 ! Aon-Woven Asbestos Felts Non-woven asbestos felts are produced in sheet formation bv carding or other fiber orienting processes. Special binders mav be added to pros ide processing strength. They are available both with and without glass doth reinforcement and are produced as sheets, tapes and rolls. Uses: These non-woven materials extend the useful range of asbestos tex tiles bv providing a strong thin felt readily saturable with resins. Thev are extensively used as basic reinforcements in both high and low pressure plastics. They also provide the basic reinforcement in impregnated as bestos tapes used as primary and secondary- insulation in high temperature resistant wire and cable. Exhibiting a strength to weight ratio unapproached bv most other avail able materials, resinated non-woven asbestos felts are finding important applications as components of rockets and missiles. Other properties which adapt them particularly to the requirements of this service are: uniform ablation, low thermal conductivity-, low thermal diffusivitv and excellent dimensional stability. Resinated asbestos felts retain a higher percentage of physical properties after exposure to extremely elevated temperatures than other inorganic reinforcements or fillers. (For test data on their performance at elevated temperatures, see page 32.) Grades: Non-svoven asbestos felts are made in standard ASTM grades, from Commercial through grade AAAA. (See Table X, page 33.) Thicknesses, Widths: Standard thicknesses range from .010" to %c". Available in xvidths from to 54". 57 Carded Asbestos Fiber Carded asbestos fiber is 100Tc asbestos which has been fiberized bypassing the crude through the several operations of the fiberizing process and by screening and carding. It is furnished in various qualities which are deter mined by the fiber length and type of crude asbestos used and by the op erations necessary to produce the carded fiber. Uses: One of the major uses of carded asbestos fibers is for the clarification of such liquids as beer, wine, oils and chemicals. The mass of tiny fibers forms a filter medium of extremely close texture which captures the un desirable suspended impurities when the liquid is allowed to pass through it. Because of the fibrous nature of asbestos, it may be opened up in pro cessing to any extent desired. Consequently, carded asbestos fibers can be furnished in many degrees of fineness to provide exactly the right screening for the liquid to be filtered. This product is also widely used as a pad for wiping excess metal from wire during manufacture and as stuffing box packing. Standard Packages: Carded asbestos fiber is packaged in 10, 25 and 50 pound cartons and in boxes containing one pound and smaller amounts. 58 d by passing >cess and by h are deterd bv the op- * clarification t tiny fibers ires the unmss through 1 up in pro4 fibers can >' the right uietal from and 50 r arronnts. ' ASTM Specifications for Asbestos Textiles Pages 60 through 96 contain the Ameri can Society for Testing and Materials specifications relating to asbestos textiles, reproduced here with the permission of the Society. These were in effect at the time this edition of the Handbook of As bestos Textiles was printed. However, since ASTM specifications are subject to continuous study and review, the reader should consult the Society's current "ASTM Standards on Textile Materials" for possible subsequent revisions. See index for subject and individual specifi cation reference. 59 f NOTE: ASTM Specifications and Methods of Test are subject to con tinual revision. Consult the Society's current "ASTM Standards on Textile Materials'' for possible changes in this specification. Standard Specifications for and Methods of Testing ASBESTOS LAP' ASTM Designation: D 1061 - 58 Adopted, 1954; Last Revised, 1958 This Standard of the American Society for Testing and Materials is issued under the fixed designation D 1061; the number immediately following the designa tion indicates the r ear of original adoption or. ir. the case of revision, the year of ki-t revision. A number in parentheses inoica'.es the year of last reapproval. -N'ote.--Editorial chance; in Sections 4 and 11 were made in October. 1959. Sections 2, 4, and 9 were revised and Section 11 on .Magnetic Rating was deleted editorially in June, 1962. Scope 1. These specifications and methods of test apply to asbestos lap a felted asbes tos product. Definition 2. Asbestos Lap is an asbestos textile product which is identified by (7) Style, (2) Type, and (3) Weight. (a) Style.--The style of asbestos lap refers to the physical construction and two distinctly different styles are nor mally available: Style I.--A ribbon-like formation of felted asbestos fiber. Style II. --A parallel assemblage of Style I lap. (b) Type. --The type of asbestos lap refers to the electrical properties of the lap as given in the Specification for1 Asbestos Textiles Used for Electrical Insulating Purposes (ASTM Designa tion: D 2100).: (c) Weight.--The weight of asbestos lap is normally expressed in the number of grains per linear yard. Grades 3. (a) The grade of asbestos lap shall be determined by the percentage of as bestos by weight, and shall conform to the following requirements: Grade Asbestos Contest. per cent Underwriters' Grade.............. Grade AAA.............................. 80 to 85, excl 85 to 90, excl 90 to 95, excl 95 to 99, excl 1 Under the standardization procedure of the Society, these specifications are under the juris* diction of the ASTM Committee D-I3 on Tex tile Materials, and are the direct responsibility of Subcommittee A-4 on Asbestos and Its Textile Products. Electrical Properties 4. Asbestos lap used for electrical insulation shall conform to the Specifica- 5 Appears in this publication. i4-a 1 r bjcct to contjndards on cation. of Testing -~ued under he rjcMjrna- . ihe year .approval. . :e d for Electrical ' ASTM Designa- -ight of asbestos -ed in the number rd. asbestos lap shall ;*rcentage of as'hall conform to ents: A*beiioi Content Pr cent SO to 85. e: R5 to 90. , 00 to 95. ( 95 to 99,, f i > ,'.'r 1 hrtrica) " sI'c<ifica- "s Specifications and Tests for Asbestos Lap (D 1061) ;on for Asbestos Textiles Used for ~iectrical Insulating Purposes (ASTM designation: D 2100).5 eight 5. Weight of asbestos lap shall conrm to the following requirements as to ermissibie variations: formance in accordance with Paragraj (a) and (b). Test Conditions 7. All test specimens shall be broug to standard condition in accordance wi Section 8 prior to testing and all te shall be conducted under standard cc ditions. Permissible Vari- i Permissible aliens in Average lariatioos in Grains per Linear> Grains per Linear \ a rd oi b ive Test] \ ard of Single . specimens, per Test specimeo, * cent per cent Style 1............... j Style II............. 1 8 5 15 10 Methods of Testlng Sampling 6. (a) Each shipment shall be divided into lots of from 800 to 1000 lb. From each lot or fraction thereof, five sample packages shall be taken at random and the tests prescribed shall be made on specimens removed from each package selected. (b) If tests from any lot fail to fall within the specified limits, two additional sets of five sample packages shall be taken from other parts of the lot and tested as before. Acceptance shall be on the basis of these two sets of five sample packages being within the required limits. (c) Optional with the purchaser, if the values determined in accordance with Paragraph (6) fail to fall within the speci fied limits, the lot shall be subdivided into units of approximately 200 lb. These shall be sampled and tested for con Standard Condition 8. Standard condition of asbestos li shall be that reached by the lap when moisture equilibrium with a standa: atmosphere having a relative humidi of 50 per cent at 21 C (70 F). A toleran of 2 per cent is permitted in relath humidity and 1.1 C (2 F) in temper; ture (Note). Note.--For purposes of tests, it is reco nized that specimens reach moisture equilibria after exposure for at least 4 hr unless otherwi: specified, under above conditions. Asbestos Content 9. The asbestos content shall be detei mined in accordance with the Method o Test for Asbestos Content of Asbesto Textile Materials (ASTM Designation D 1918).= Weight 10. From each of five packages selectee in accordance with Section 6, a 1-yd tes: specimen shall be taken. Care shall b< taken that the specimen is not scuffed oi torn, and for this reason the outer wrap of the lap shall be removed before taking the specimen. Each specimen shall be weighed to the nearest grain, and the average weight of the five specimens cal culated. NOTE: ASTM Specifications and Methods of Test are subject to con tinual revision. Consult the Society's current "ASTM Standards on Textile Materials" for possible changes in this specification. Standard Specifications and Methods of Test for ASBESTOS ROVING1 ASTM Designation: D 375 - 59 Adopted, 1936; Last Revised, 1959 This Standard of the American Society for Testing and Materials is issued under the fired designation D 375; the final number indicates the year of orig inal adoption as standard or, in the case of revision, the year of last revision. Note.--Editorial changes in Sections 2, S, 9, and 10 were made June, 1960; also the Notes were numbered. Editorial changes throughout the method were made in June, 1962. Scope 1. These specifications and methods of test apply to asbestos roving, used mostly as the main component of heat-resistant electrical insulation for various types of wire and cable. Two types are covered as defined in Section 2(a) and (b). Definitions 2. (a) Asbestos Roving.--An assem blage of carded asbestos, with or without other fibers, rubbed into a single strand without twist. (6) Reinforced Asbestos Roving.--As bestos roving containing a core of other fibers. (c) Standard Condition. -- Standard condition of asbestos roving shall be that reached by the roving when in moisture equilibrium with a standard atmosphere having a relative humidity of 1 Under the standardization procedure of the Society, these specifications are under the juris diction of the ASTM Committee D-13 on Tex tile Materials, and are the direct responsibility of Subcommittee A-4 on Asbestos and Its Textile Products. 50 per cent at 70 F (21 C). A tolerance of 2 per cent is permitted in relative humidity and 2 F (1.1 C) in tempera ture. Note.--For purpose of tests, it is recognized that specimens reach moisture equilibrium after exposure to moving air for at least 4 hr, unless otherwise specified, under the above conditions. (d) Number (Cut).--A number hy phenated with the word "cut" indicates the number of 100-yd units in 1 lb of a standard asbestos roving, and desig nates the cut-number of that roving. Number (Cut) 3. (a) The standard number of asbes tos roving is designated as "cut." The yards per pound of the standard cuts shall conform to the requirements as prescribed in Table I. Note 1.--The tolerances on special numbers such as 5)-cut. 6j-cut, etc. shall be equal to those of the standard numbers. (b) The cut of reinforced asbestos roving shall be determined without re moving the reinforcing core yam. n-w t to conlards on >n. issued ' origision. ). A tolerance ed in relative ) in tempera- i is recognized , _ilibrium after rut 4 hr, unless jove conditions. number hyut" indicates s in 1 lb of a . and desigat roving. ber of asbes: "cut." The andard cuts -irements as 7?*1 "umbers 1 ** equal to asbestos ' 'ihout re irn. Specifications and Tests for Asbestos Roving (D 375) Grades 4. (a) The grade of asbestos roving mall be determined by the percentage of -ibestos by weight, and shall conform to .he following requirements: Grade Underwriters' grade................ Grade A...................................... Grade AA................................... Grade AAA................................ Asbestos Contest, per cent 80 to 85, excl 85 to 90, eicl 90 to 95, excl 95 to 99. excl TABLE I. -- REQUIREMENTS FOR YARDS PER POUND OF STANDARD ASBESTOS ROVING. 17 >| i Cut Number 5^ i o-- 2< jU s <N 9 SGJ*>"0 VZa e Zi>i. - j: v e h. *** 3.2 a.g vlU e o.Eji Q5m -' 5-cut......... 600 460 to 640 425 to 675 6-rut........ COO 552 to 648 510 to 690 7 -cut......... 700 644 to 756 595 to 805 S-cut ... 600: 736 to 664 680 to 920 9-cut......... 900: 82S to 972 765 to 1035 10-cut......... 1000: 920 to 1080 850 to 1150 12-cut........ 1200! 1104 to 1296 1020 to 13S0 M-cut......... 1400! 12SS to 1512 1190 to 1610 16-cut........ 1COO! 1472 to 1728 1300 to 1840 18-cut......... 1800! 1656 to 1944 1530 to 2070 20-cut......... 20001 1840 to 2160 1700 to 2300 22-cut......... 2200! 2024 to 2376 1870 to 2530 24-cut........ 2400i 2208 to 2592 2040 to 2760 26-cut......... 2600 i 2392 to 2808 2210 to 2990 28-cut......... 2800] 2576 to 3024 2380 to 3220 30-cut......... 30001 2760 to 3240 2550 to 3460 35-cut......... 3500! 3220 to 3780 2976 to 4025 40-cut......... 4000! 3680 to 4320 3400 to 4600 45-cut......... 4500! 4140 to 4860 3825 to 6176 60-cut......... 5000! 4600 to 5400 4250 to 6750 Methods of Testing Sampling 6. (a) Each shipment shall be divided into lots of from 800 to 1000 lb. From each lot or fraction thereof, five sample cones shall be taken at random and the tests prescribed shall be made on speci mens removed from each package se lected. (b) If tests from any lot fail to fall within the specified limits, two additional sets of five sample cones shall be taken from other parts of the lot and tested as before. Acceptance shall be on the basis of these two sets of five sample cones being within the required limits. (c) Optional with the purchaser, if the values determined in accordance with Paragraph (b) fail to fall within the speci fied limits, the lot shall be subdivided into units of approximately 200 lb. These shall be sampled and tested for con formance in accordance with Paragraph! (a) and (b). Test Conditions 7. All test specimens shall be brought to a standard condition in accordance with Section 2 (c) prior to testing and all tests shall be made under the standard condition. Note 2.--The 16- and 18-cut rovings are available only in the Underwriters' grade: all other cuts are available in all four grades. (b) The asbestos content of reinforced asbestos roving shall be determined with out removing the reinforcing core yam. Electrical Properties 5. Asbestos roving used for electrical insulation shall conform to the Specifi cation for Asbestos Textiles Used for Electrical Insulating Purposes (ASTM Designation: D 2100).! * Appears in this publication. Number (Cut) 8. (a) Number of Tests.--Make ten de terminations of the number of yards per pound on each set of five packages se lected. (6) Procedure.--Group the packages on the floor and draw five strands from them slowly, looping over a support to as semble 20 strands, which shall be cut into a 1-yd length while suspended. Weigh the 20 yd to the nearest 0.1 grain and calculate the number of yards per pound from the following formula: (D 375) asbestos content in Method of Test for of Asbestos Textile esignation: D 1918).5 ! ` | Appnnvpn ar AMERICAN STANDARD LH.18-1961T BY AMERICAN STANDARDS ASSOCIATI UDC 677.31:620.1 NOTE: This Specification is scheduled for revision hv the ASTM in 1967 to conform with the class designations for Asbestos Yam as shown on paes 3S and 39 of this edition of the Handbook. Standard Specifications a?i d Methods of 'Vest for ASBESTOS YARNS** ASTM Designation: D 299 - 60 Adopted 1954; Revised, I960.' This StanJ.ird of the American Society lor Testing and Materials is issued under the fixed designation D 299; the final number indicates the year of orig inal adoption as standard or, in the case of revision, the year of last revision. Note.--Section 8 was added and Sections 2, 11, and 14 were revised editorially in June, 1962. Scope (b) Plain Asbestos Yarn.--Plain 1. These specifications define asbestos bestos yarn consists of: (1) asbes yarn, prescribe the methods of testing, fiber, or (2) asbestos and other fib* i and stipulate tolerances. (c) Metallic Asbestos Yarn.--Meta f asbestos yarn consists of plain ast i Definitions tos yarn or roving twisted with br; % 33 2. (a) Asbestos Yarn.--A twisted copper, or other fine wire. It is a i assemblage of; (/) asbestos fiber, (2) termed "wire-inserted yam." f i asbestos and other fibers, (3) asbestos (d) Reinforced Asbestos Yarn.--Pi } and other fibers and wire, or (4) asbestos asbestos yam or roving twisted w and other fibers with an insert of cotton an insert of yam made of other fibers or other yam reinforcement. (e) Standard Condition.--Stand; 1 Under the standardization procedure of the Society, these specifications are under the juris diction of the ASTM Committee D-13 on Textile Materials, and are the direct responsibility of Subcommittee A-4 on Asbestos and Its Textile Products. * Prior to their present adoption as standard, these specifications were published as tentative from 1928 to 1929. They were adopted in 1929, published as standard from 1929 to 1941, being revised in 1933, 1936. and 1937, Dut withdrawn and replaced in 1941 by Tentative Specifica tion* D 299 - 40 T which were published as tentative from 1940 to 1942. They were again adopted in 1942 and published os standard from 1942 to 1948. They were reverted to tentative in 194S, and were published as tentative from 1948 to 1954. being revised in 1949. 1950. 1951. and 1952. condition of asbestos yam shall be tl reached by the yam when in moist equilibrium with a standard atmosph having a relative humidity of 50 per c at 70 F (21 C). A tolerance of 2 ] cent is permitted in relative humid and 2 F (1.1 C) in temperature. Note.--For purpose of tests, it is recogni that specimens reach moisture equilibrium a exposure for at least 4 hr, unless otherwise sp fied, under the above conditions. (/) Tvrist, Direction of.--A yarn ha Specifications and Tests for Asbestos Yarns (D 299) twist if, when held in a vertical posi tion, the spirals around its central axis conform in direction of slope to the central portion of the letter "S," and Z twist if the spirals conform in direc tion of slope with the central portion of the letter `Z." Note --This definition applies to the twist in single yams the ply twist in plied yarns, and the cable or hawser twist in cords. (J) Tarn Construction.--Based en cut as defined in Paragraph (g), as!--' yams are designated in the a?br textile industry by numbers which . cate the cut-number, the numb-: plies, and whether the yam is pia--. TABLE 1.--REQUIREMENTS YARDS PER POUND OF STAND. SINGLE ASBESTOS YARNS. Cut Number li*5 Permissible Variations in Averare Yards per Pound Per-- Variv. YiT ** Poucd" 30-yd ' * z (g) Cut (Asbestos).--A term derived by cutting (dividing) 7000 grains into linear mass units by the grain weight of 100 yd of a single yarn. The number of such units expresses the number of the cut and, when multiplied by 100, indi cates the nominal yards per pound. 6-cut............. 500 460 to 540 425 u 6-cut............. 600 652 to 648 510 t- 7-cut............. 700 644 to 756 595 i-> 8-cut............. SOO 738 to 864 6S0 : 9-cut............. 900 82S to 972 765 tr 1000 920 to 10S0 S50 t 12-cut............. 1200 1104 to 1296 1020 14-cut............. 1400 12SS to 1512 1190 ; , . 16-cut............. 1600 1472 to 1728 1360 tu ' 1800 1A5A tn 1044 1530 to . 20-cut............. 2000 1840 to 2160 1700 to v 22-cut............. 2200 2024 to 2376 1870 to 2i-v 24-cut............. 2400 220S to 2592 2040 io::t? 26-cut............. 2600 2392 to 2S08 2210 to 2."5 28-cut............. 2S00 2576 to 3024 2380 to 3775 30-cut............. 3000 2760 to 3240 2550 to 34.--o 3500 3220 to 3780 2976 to 41-3 40-cut............. 4000 3680 to 4320 3400 to 46*5 45-cut............. 4500 4140 to 4860 3825 to 51 > 50-cut............. 5000 4600 to 6400 4250 to S7S5 Example.--If five 30-yd skeins of single yarn, or 150 yd, weigh 637.5 grains, then 100 yd weigh 425 grains. metallic. All yams comprising 5-cut to 9-cut, inclusive, have 3-digit construction -- 16.47, or 16.47-cut, which is 16-cut on 425 the light side; and 16 X 100 -- 1600 nominal yd per lb. (h) Ply.--Ply is the number of strands of single asbestos yam twisted together to form a heavier yam. Ply is a term used principally in combination with a number to designate the strands of single yam twisted together, as 2-ply, 3-ply, etc. () Number (Cut).--A number hy phenated with the word cut indicates the number of 100-yd units in 1 lb of a stand ard asbestos yam, and designates the cut-number of that yarn. numbers; yams comprising 10-cut to 50-cut, inclusive, have 4-digit construc tion numbers. Digits are significant as follows: The last digit, if zero, indicates yam; if the last digit is 1, 2, or 3, ifc* number of strands of wire twisted with the asbestos is designated. The next to last digit designates thf plies. The remaining digits (1 or 2) designate the cut-number. Examples: No. 931 yarn........ No. 1010 yarn........ No. 1420 yam........ 9-cut, 3-ply--1 witty*** 10-cut, single, plain y*** 14-cut, 2-ply, plain 1*** TH-t* cc 5-- * * i A > * * 3 (D 299) sction.--Based on the iragraph (g), asbestos ted in the asbestos numbers which indiber, the number of the yarn is plain or 3UIREMENTS FOR .VD OF STANDARD YARNS. 'ermissible ariations in trice Yards ;<r Pound Permissible Variations in Yards per Pound of Single JO-jrd Skein 60 to M0 .52 to M8 44 to 766 36 to 864 28 to 872,1 425 to 576 510 to 690 695 to 805 6S0 to 920 765 to 1035 20 to 10S0! S50 to 1150 04 to 1296' 1020 to 1380 S8 to 1612) 1190 to 1610 72 to 1728 1360 to 1840 .56 to 19441 1530 to 2070 40 to 2160j 1700 to 2300 '24 to 2376 1870 to 2530 08 to 2592! 2040 to 2760 92 to 2808' 2210 to 2990 ,76 to 30241 2380 to 3220 60 to 3240! 2550 to 3450 20 to 3780; 2976 to 4025 BO to 4320 3400 to 4600 40 to 4860 3825 to 5175 00 to MOO] 4250 to 5750 comprising 5-cut to e 3-digit construction imprising 10-cut to ive 4-digit construets are significant as zero, indicates plain ;it is 1, 2, or 3, the if wire twisted with plated. digit designates the its (1 or 2) designate f J 1 V ' \ j 1 1 1 1 1 j I 1 7-cut, 3-ply-l wire yam 3-cut, tingle, plain yam 4-cut, 2-p)y, plain yarn Specifications and Tests foe Asbestos Yarns (D 299) Breaking Strength 3. The breaking strength of asbestos am shall be expressed in pounds and decimal fractions thereof and shall con'orm to: (I) The specified average for the ship ment. (J) The allowed minus variation of :r.e average, and (J) The minimum specified for any individual break. Grade Asbestos Cootest Commercial Grade___ 76 to 80 per cent, excl Underwriter*'Grade.. 80 to 85 per cent, excl Grade A..........................85 to 90 per cent, excl Grade AA...................... 90 to 95 per cent, excl Grade AAA................... 95 to 99 per cent, excl Grade AAAA................ 99 to100 per cent, incl (b) The asbestos content of reinforced asbestos yam shall be determined with out removing the reinforcing core yam. (c) The asbestos content of metallic asbestos yam shall be determined after the wire has been removed. Yards Number (Cut) Electrical Properties 4. (a) The yards per pound of the standard single asbestos yams shall con form to the requirements as prescribed in Table I. (b) The cut of reinforced asbestos yam shall be determined without removing the reinforcing core yam. (c) The yards per pound of metallic asbestos yam is less than that of plain yam of the same cut in proportion to the weight of the inserted wire. (d) The yards per pound of sized yam, single or plied, shall be subject to an additional tolerance of --2 per cent in comparison with the corresponding un treated yam. Size of Wire 5. The diameter of the wire used in metallic asbestos yam shall not vary from the size specified by more than 0.001 in. Twist 6. The directions and turns per inch of twist shall be as mutually agreed upon by the manufacturer and the pur chaser. Grades 7. (a) The grades of plain, metallic, and reinforced asbestos yam shall be determined by the percentage of asbestos content by weight, and shall conform to the following requirements: 8. Yams used for electrical insulation shall conform to the Specifications for Asbestos Textiles Used for Electrical Insulating Purposes (ASTM Designa tion: D 2100).* Methods of Testing Test Conditions 9. All test specimens shall be brought to a standard condition in accordance with Section 2 (e) prior to testing, and all tests shall be made under the stand ard condition. Sampling 10. (a) Unless otherwise specified, each shipment shall be divided into lots of 800 to 1000 lb. From each lot, or fraction thereof, five sample tubes shall be taken at random, preferably from more than two cases, and the tests prescribed for strength and yardage (Sections 11 and 12) shall be made on specimens from each package taken. (b) If tests from any lot fail to fall within the specified limits for strength and yardage, two additional sets of five sample tubes each shall be taken from other parts of the lot and tested as be fore. Acceptance for breaking strength and yardage tests shall be on the basis of these two additional sets of five sample tubes being within the required limits. * Appear* in this publication. Specifications kkv Tests for Asbestos Yarns (D 299) (c) Optional with the purchaser, if the or, the average of any five tests at random should values as determined in accordance with be not leu than 2.56 lb. Paragraph (5) fail to fall within the speci fied limits, the lot shall be subdivided into Yarn Number (Cut) units of approximately 200 lb. These shall be sampled and tested for conform ance in accordance with Paragraphs (a) and (b). 12. The cut of plain or reinforced as bestos yam, single or plied, shall be calculated by dividing by 100 the yards per pound as determined in accordance Breaking Strength with Paragraphs (a) to (c). () The yards per pound of plain or 11. (c) Apparatus.--A tensile testing reinforced single asbestos yam shall be machine conforming to the Specifications determined by reeling a 30-yd skein for Textile Testing Machines (ASTM from each of five tubes taken at random Designation: D 76).J from each lot of 800 to 1000 lb. These (b) Procedure.--All tests shall be made five skeins shall be conditioned for at on single strands. Single strands shall be Ieast4 hrin accordance with Section 2 (e), broken after conditioning the tubes for and the weight of each skein shall then 12 br in accordance with Section 2 (e). A single-strand tester of proper capacity, with the clamps set 10 in. apart and having a speed of pulling clamp of 12 $ in per min, shall be used. One break shall be made from each tube of each set of five tubes selected in accordance with be determined to the nearest grain. The average yards per pound shall be the arithmetical average of the five deter minations, calculated as follows: 7UOU x 30 Y~ w Section 10. Care shall be taken to avoid loss of twist during the test. The holding device shall be of the drum or capstan type. All breaks within 5 in. of the con tact points shall be discarded. (c) Calculation and Report.--The al lowed variation from the average of five individual tests shall be calculated as follows: where: Y = yards per pound, and W -- weight in grains of a 30-yd skein. () The yards per pound of plied plain or reinforced asbestos yam shall be deter mined by reeling a 30-yd skein from each of five tubes taken at random from each lot of 800 to 1000 lb. These five skeins shall be conditioned for at least 4 hr in V accordance with Section 2 (e), and the weight of each skein shall then be deter where: T = allowed minus variation of the average of any five tests and the specified average, and V -- spread between the specified mini mum of any single break and the mined to the nearest grain. The average yards per pound shall be the arithmetical average of the five determinations, cal culated as follows: y ^ 7000 X 30 X (number of plies) W X 0.95 specified lot average. where: Example.--Assumed that the specified aver age is 3 lb and minimum break is 2 lb, then F = yards per pound of single ply, W = weight in grains of a 30-yd skein, and 0.95 = factor to compensate for an aver age contraction of 5 per cent in r - 0.44 curred in twisting. 68 (D 299) * test* at random should I .in or reinforced asor piied, shall be -g by 100 the yards :ined in accordance to (c). pound of plain or estos yam shall be big a 30-yd skein ss taken at random to 1000 lb. These conditioned for at s with Section 2 (e), ;h skein shall then nearest grain. The rand shall be the vi the five deter..5 follows: X .'0 T d. and s of a 30-yd skein, ound of plied plain yam shall be dcter-yd skein from each random from each . These five skeins "or at least 4 hr in ion 2 (), and the -hall then be deter-rain. The average be the arithmetical ^terminations, cal- nutnber of piirO <095 ~ 'd of Sing|c ply, Jins of a 30-yd ""sate for an aver) of 5 per cent ^ *ng. 4- Specifications and Tests foe Asbestos Yaens (D 299) (c) The yards per pound of metallic asbestos yam, single, or plied, shall be determined by reeling a 30-yd skein from each of five tubes taken at random from each lot of 1000 to 1400 lb. These five skeins shall be conditioned for at feast 4 hr in accordance with Section 2 (t), and the weight of each skein shall then be determined to the nearest grain. The weight in grains of the wire taken from one skein shall be determined. This weight shall be subtracted from the weight of each skein. The average yards per pound shall be the arithmetical average of the five determinations, cal culated as follows: 7000 X 30 X (number of plies) Y" ' X 0.95 where: Y = yards per pound, W = weight in grains of 30-yd skein (without wire), and 0.95 = factor to compensate for an aver age contraction of 5 per cent in curred in twisting. Twist 13. (a) Direction of Twist.--The di rection of twist shall be determined in accordance with Section 2 (f). (6) Turns in Single Yarn.--The turns per inch of twist in single yam shall be determined on any standard single yam twist tester. The first 2 yd of any pack age of yam shall be discarded, and all possible care shall be exercised in han dling samples to prevent a change in the existing twist. The yam, drawn just taut enough to prevent sagging, shall be gripped in the twist counter with clamps set 4 in. apart. One clamp shall be ro tated until the twist is removed as indi cated by the yam breaking under its own weight, or by visual examination of the sample. The twist of yam in a shipment shall be the average of three tests from each of the five tubes or bobbins selected in accordance with Section 10 (a). (c) Turns in Plied Yarn.--The turns per inch of twist in plied yam shall be determined as described in Paragraph (b), with the following exception: The clamps shall be set 10 in. apart. Asbestos Content 14. (a) Determine the asbestos con tent in accordance with the Method of Test for Asbestos Content of Asbestos Textile Materials (ASTM Designation: D 1918).5 (b) In making asbestos content deter minations on asbestos yams reinforced with continuous filament glass yams, such insertion shall be removed before making the determination. The organic content shall be computed on the basis of the oven-diy weight of the glass rein forced yam previous to removal of the glass yam insert. APPROVED AS AMERICAN STANDARD L14.U3.19M NT AMERICAN STANDARDS ASSOCIATION NOTE: ASTM Specifications and Methods of Test are subject to con tinual revision. Consult the Society's current "ASTM Standards on Textile Materials" for possible changes in this specification. Tentative Specification and Tolerances for WOVEN ASBESTOS CLOTH1 ASTM Designation: D 1571 - 66 T Issued, 1958; Revised, 1966 This Tentative Specification has been approved by the sponsoring committee and accepted by the Society in accordance with established procedures, for use pending adoption as standard. Suggestions for revisions should be addressed to the Society at 1916 Race St., Philadelphia, Pa. 19103. 1. Scope 3. Classification 1.1 This specification covers woven asbestos cloth having a minimum of 75 per cent asbestos fiber by weight, ex cluding the weight of other inorganic reinforcing strands which may be pres ent. Note 1--Specifications for asbestos yarns are covered in ASTM Specification D 299, for Asbestos Yam.' 2. Definitions 2.1 Asbestos Fiber, n.--For purposes of this specification, asbestos fiber is the hy drous magnesium silicate serpentine mineral identified as chrysotile and having the general empirical formula Mg,SiA(OH),. 2.2 For definitions of other terms used in this specification, refer to ASTM Def initions D 123, Terms Relating to Tex tile Materials.* * 1 Under the standardization procedure of the Society, this specification is under the jurisdiction of the ASTM Committee D-13 on Textile Materials, and is the direct responsi bility of Subcommittee A-4 on Asbestos and Its Textile Products. * Appears in this publication. 3.1 The classes of asbestos doth are based on the nature of the yams from which they are woven. 3.1.1 Class A--Cloth constructed of asbestos yarns containing no reinforcing strands. 3.1.2 Class --Cloth constructed of asbestos yams containing wire reinforce ment. 3.1.3 Class C--Cloth constructed of asbestos yarns containing organic rein forcing strands. 3.1.4 Class D--Cloth constructed of asbestos yams containing non-metallic inorganic reinforcing strands. 3.1.5 Class E--Cloth constructed of two or more of the yams used in cloth classes A through D. 3.2 Grades--The grades of asbestos cloth are based on the percentage of as bestos content by weight as stated in Table 1. 4. Basis of Purchase 4.1 Woven asbestos cloth is normally purchased on the basis of class, grade, weave, weight, thickness, and width as O-M *7A APPROVED AS V STANDARD LU.m-1%6 STANDARDS ASSOC1ATIOH e subject to conM Standards on reification. a?ices for Specification and Tolerance for Woven Asbestos Cloth (D 1571) j -..lrmally furnished in rolls of 50 or 100 6.1.2 Thickness--The thickness of as i yards (45 or 90 m). bestos cloth shall be within the following limits: 5. Materials and Manufacture Nominal Thickness Permissible Limits 5.1 Yarn--Asbestos cloth shall be uni'rr.'.ly woven from a specified grade of fbestos yarn with or without reinforce.-.ent. 5.2 Wire Reinforcements--The wire reforcenient may be brass, copper, zinc, .r other metal or alloy as specified in the 0.050 in. (1.27 mm) and under............. Over 0.050 in. (1357 mm) ..................... 0.005 in. (0.12 mm) f+0.010 in. (0.25 mm) (--0.005 in. (0.12 mm) 6.1.3 Weight--The weight of asbestos cloth shall be within 7 per cent of the specified weight. ,rder. TABLE 2--LOT SAMPLE. ?onng commitied procedures, visions should ia, Pa. 19103. of asbestos cloth are ure of the yams from ven. -Cloth constructed of ntaining no reinforcing -Cloth constructed of i raining wire reinforce- Cloth constructed of ntaining organic rein- - Cloth constructed of ntaining non-metallic ng strands. Cloth constructed of e vams used in cloth D. grades of asbestos the percentage of asweight as stated in tos cloth is normally 1 nsis of class, grade, kness, and width as O-M TABLE 1--GRADES OF WOVEN ASBESTOS CLOTH. Number of Rolls ia Lot or Shipment Number of Rolls to be Taken for Test Grade Asbestos Conteot, weight per cent i........................................ 2 to 8............................... i 2 9 to 15............................. 3 . orcmerciai................... 16 to 40........................... 4 Underwriters................ A...................................... 41 to 65........................... 5 66 rolls and over........... 10 per cent of shipment .VA.................................. . . . . 90 to 95, eicl rounded off to the * AAA................................ next higher integer AAAA............................ .. . . 99 to 100, incl 6.1.4 Fabric Count--The warp ends or 5.3 Organic Reinforcements--The or filling picks shall be within the following ganic reinforcements may be cotton, limits: nylon, rayon or other spun or filament Ends or Picks per inch Permissible Limits yarns as specified in the order. 20 or less per inch......... 1 end or pick per * 5.4 Inorganic Reinforcements--The in inch i1I organic reinforcement may be glass, or other ceramic or vitreous spun or filament More than 20 per inch (25 mm)................... 5 per cent of the specified count. ia yams as specified in the order. 6.1.5 Yarn Number (Cut)--The yarn 6. Physical Requirements and Toler ances 6.1 The physical properties of woven asbestos cloth shall conform to the re quirements as specified in the order, sub ject to the following tolerances: 6.1.1 Width--The width of asbestos cloth shall be within the following limits: number (cut) shall be as specified and shall conform to the requirements stated in ASTM Specification D 299.* 6.1.6 Asbestos Content--The asbestos content of the particular grade specified shall conform to the limits stated in Table 1. 6.1.7 Breaking Strength--The break ing strength (breaking load) of asbestos Nominal Width Up to and including 40 in. (1 m).................... Over 40 in. up to and including 60 in. (1.5 m)............................... Over 60 in...................... Permissible Limits 0.5 in. (12 mm) 0.75 in. (19 mm) 1.00 in. (25 mm) cloth shall be as agreed upon between the buyer and seller. 6.1.8 Electrical Properties--Cloth to be used for electrical insulating purposes shall conform to the requirements in ASTM Specification D 2100, Asbestos Specification and Tolerance for Woven Asbestos Cloth (D 1571) Textiles Used for Electrical Insulating of all measurements as the average thick Purposes.* ness of the lot. Make no measurement 7. Sampling 7.1 From each lot of cloth, take a lot within 3 in. (76 mm) of any edge of the specimen, and distribute the places of measurement approximately uniformly sample in a random manner to be rep over the specimen. resentative of the lot in accordance with the schedule in Table 2. Cut a specimen from each roll taken for test, each speci men to be the full width of the roll and at least 0.5 yd (0.5 m) long. The specimen may be taken from the cut end of the roll. 9.3 Weight--From each roll taken for test, cut a specimen not less than 0.5 yd (0.5 m) in length and across the full width of the cloth, measuring the length and width of the specimen to the nearest 0.1 in. (2.5 mm) in at least three places, using a steel tape or rigid rule. Make sure that 8. Conditioning the specimen is free from tension, wrin kles, and folds. Weigh the specimen to 8.1 Condition all specimens (without the nearest 0.01 oz (0.3 g). Using the preconditioning) for a period of 4 hr, or average length and average width, calcu until the specimen shows no progressive late and report the weight in ounces per change in weight of more than 0.1 per square yard (kilograms per square meter) cent after an exposure of 0.5 hr, in an at on the basis that the weight per square mosphere having a relative humidity of yard (square meter) of the lot of cloth is 50 2 per cent at 70 2 F (21 1.1 C). equivalent to the arithmetic mean of the 9. Methods of Test results. 9.4 Fabric Count--Determine the fab 9.1 Width--Measure the width of the ric count on one or more specimens from cloth, either on the full roll or on a short each roll taken for test, as directed in specimen from each roll taken for test, as ASTM Method D 1910. directed in ASTM Methods D1910, Tests for Construction Characteristics of Woven Fabrics.* 9.2 Thickness--Measure the thickness 9.5 Asbestos Content--Determine the asbestos content on one or more speci mens from each roll taken for test as di rected in ASTM Method D 1918, Test of the cloth as directed in ASTM Method for Asbestos Content of Asbestos Textile D 1777, for Measuring Thickness of Tex Materials.* tile Materials.* Use a gage of the dead 9.6 Breaking Strength (Load)--Deter weight type equipped with a dial gradu mine the breaking load by the grab ated to read directly to 0.001 in. (0.025 method as directed in ASTM Method mm), and having a circular presser foot D 1682, Test for Breaking Load and with a diameter of 0.375 0.001 in. Elongation of Textile Fabrics.* Use a (9.5 0.025 mm). The presser foot and CRT--constant rate of traverse type ten moving parts connected therewith shall sile testing machine operated at 12 0.5 be weighted so as to apply a total load of in. (305 12 mm) per minute. If agreed 6 0.1 oz. (170 3 g) equivalent in upon between the buyer and seller, a pressure to 3.4 psi (0.24 kg/cm*) to the CRE--constant rate of elongation type specimen. Make ten thickness measure machine may be used. ments on a specimen from each roll taken for test and report the calculated average 10. Conformance 10.1 If the test results for the lot con *1066 Book of ASTM Standard#. Fart 24. form to the requirements for all charac- *70 -LOTH (D 1571) as the average thickike no measurement i) of any edge of the ribute the places of >ximately uniformly 1 each roll taken for not less than 0.5 yd ' across the full width ring the length and an to the nearest 0.1 st three places, using rule. Make sure that from tension, wringh the specimen to (0.3 g). Using the verage width, calcuveight in ounces per ns per square meter) ? weight per square if the lot of cloth is .hmetic mean of the Determine the fab-.ore specimens from test, as directed in i0. it--Determine the one or more spedaken for test as dithod D 1918, Test of Asbestos Textile 'tk (Load)--Deter:oad by the grab n ASTM Method eaking Load and e Fabrics.* Use a traverse type ten*erated at 12 dt 0.5 minute. If agreed 'yer and seller, a f elongation type j | ]i j M \ j * : i > 7 for Jot con,s for all charac- *-44 Specification and Tolerance for Woven Asbestos Cloth (D 1571) eristics listed in 6.1.1 through 6.1.8 inclusive, the lot shall be considered ac ceptable. 10.2 If the test results for one or more characteristics do not conform to the requirements, take a new laboratory sam ple from either the original lot sample or a new lot sample. Test the new sample ;`jr the characteristic(s) that did not con form to the requirements in the first test and average the results of the first a second samples as if they were one test double the original number of specime If the new average(s) conform (s) to t specified requirements, the lot shall considered acceptable. 10.3 If the test results obtained as rected in 10.2 do not conform to t specified requirements, the lot shall considered unacceptable. 62-451 NOTE: ASTM Specifications and Methods of Test are subject to con tinual revision. Consult the Society's current "ASTM Standards on Textile Materials" for possible changes in this specification. Tentative Specification and Tolerances for WOVEN ASBESTOS TAPE1 ASTM Designation: D 315 - 66 T Issued, 1958; Last Revised, 1966 This Tentative Specification has been approved by the sponsoring commit tee and accepted by the Society in accordance with established procedures, for use pending adoption as standard. Suggestions for revisions should be addressed to the Society at 1916 Race St., Philadelphia, Pa. 19103. 1. Scope 1.1 This specification covers woven as bestos tape ha%'ing a minimum of 75 per cent asbestos liber by weight, excluding the weight of other inorganic reinforcing strands which may be present. Note 1--Specifications for asbestos yams are covered in ASTM Specification D 299, for Asbestos Yam,* 2. Definitions 2.1 Asbestos Fiber, n.--For purposes of this specification, asbestos fiber is the hydrous magnesium silicate serpentine mineral identified aschrysotileand having the general empirical formula MgjSijO*(OHh. 2.2 For definitions of other terms used in this specification, refer to ASTM Def initions D 123, Terms Relating to Textile Materials. tapes are based on the nature of the yarns from which they are woven. 3.1.1 Class A--Tape constructed of asbestos yarns containing no reinforcing strands. 3.1.2 Class B--Tape constructed of asbestos yarns containing wire reinforce ment. 3.1.3 Class C--Tape constructed of as bestos yarns containing organic reinforc ing strands. 3.1.4 Class D--Tape constructed of asbestos yarns containing non-metallic inorganic reinforcing strands. 3.1.5 Class E--Tape constructed of two or more of the yarns used in tape dasses A through D. 3.2 Grades--The grades of asbestos tape are based on the percentage of as bestos content by weight as stated in Table 1. 3. Classification 3.1 Classes--The classes of asbestos 1 Under the standardization procedure of the Society, this specification is under the jurisdic tion of the ASTM Committee D-13 on Textile Materials, and is the direct responsibility of Subcommittee A-4 on Asbestos and Its Textile Products. * Appears in this publication. 4. Basis of Purchase 4.1 Woven asbestos tape is normally purchased on the basis of dass, grade, weight, width, length, and thickness as specified in the order. 4.2 Rolls of asbestos tape are normally furnished in the following lengths: nm c yarns led of -.forcing ted of inforced of asinforctcd of metallic ted of n tape bestos of asied in mally rade, * as illy Specification for Woven Asbestos Tape (D 315) Nomin&J Thickness Nominal Roll Length Up to and including 0.03 in. (0.76 ram)................. 36 yd (33 m) Over 0.03 in. up to and in cluding H6 in. (1.6mm). 100 ft (30 m) Over Efj in.......................... 50 or 100 ft (15 or 30 m) 4.3 Special roll lengths shall be as agreed upon between the buyer and seller. 4.4 At least 90 per cent of the number of rolls in the lot shall be furnished as one oiece. N'o roll shall contain more than two nieces. The shortest piece shall not be .'ess than 20 per cent of the specified .-.ominal roll length. asbestos tape shall conform to the re quirements as specified in the order, sub ject to the following tolerances: 6.1.1 Width--The width of asbesto: tape shall be within the following limits Nominal Width Permissible Limits Up to and including 1 in. (25.4 mm)............. K6 (1.6 mm) Over 1 in. up to and in cluding 3 in. (76 mm). in. (2.4 mm) Over 3 in.......................... t in. (3.2 mm) 6.1.2 Thickness--The thickness of as bestos tape shall be within the following limits: TABLE 1--GRADES OF WOVEN ASBESTOS TAPE. Grade Asbestos Content, weigh; per cent Commercial.................. . . . . Underwriters................ . . . . A...................................... .. . AA ................... AAA............................... . . . . AAAA............................ . .. . 75 to 80, excl 80 to 85, excl $5 to 90, excl 95 to 99, excl 99 to 100, incl Nornin*) Thickness Permissible Limits Up to and including 0.03in. (0.76jnin). 0.003 in. (0.07 mm) Over 0.03 in. up to and including 3-lc in. (1.6 mm)......... 0.005 in. (0.12 mm) Over %6 in............... f+0.010 in (0.25 mm) \ -- 0.005 in. (0.12 mm) 6.1.3 Weight--The weight of asbestos tape shall be within 10 per cent of the specified weight. 5. Materials and Manufacture 6.1.4 Fabric Count--The total number 5.1 Yarn--Asbestos tape shall be uni of warp ends and filling picks per inch formly woven from a specified grade of shall be within the following limits: .4 asbestos yarn with or without reinforce Tout Wsrp Ends Permissible Limits ment. 5.2 Wire Reinforcement--The wire re inforcement may be brass, copper, zinc, or other metal or alloy as specified in the order. 5.3 Organic Reinforcement--The or All widths........................ 10 per cent of the specified number of ends. Picks per lock 20 or less per inch (25 mm).............................. 1 pick per inch More then 20 per inch.. 5 per cent of the ganic reinforcement may be cotton, ny lon, rayon,or other spun or filament yarns specified filling count. as specified in the order. 6.1.5 Yarn Number (Cut)--The yam 5.4 Inorganic Reinforcement--The in number (cut) shall be as specified and organic reinforcement may be glass, or shall conform to the requirements stated other ceramic or vitreous spun or filament in ASTM Specification D 299.1 i yarns as specified in the order. 6.1.6 Asbestos Content--The asbestos i 5.5 It is permissible to use a maximum content of the particular grade specified i of two ends of yarn other than asbestos shall be in accordance with the limits in each selvage. stated in Table 1. 6. Physical Requirements and Toler ances 6.1.7 Breaking Strength--The break ing strength (breaking load) of asbestos tape shall be as agreed upon between the 6.1 The physical properties of woven buyer and seller. Specification for Woven Asbestos Tape (D 315) 6.1.8 Electrical Properties--Tape to be used for electrical insulating purposes shall conform to the requirements in ASTM Specification D 2100, for As bestos Textiles Used for Electrical In sulating Purposes.1 7. Sampling 7.1 From each lot of tape, take a lot sample in a random manner to be rep resentative of the lot in accordance with the schedule in Table 2. Cut a specimen from each roll taken for test, each speci men to be the full width of the tape and at least 5 ft. (1.5 m) long. The specimen may be taken from the cut end of the roll. TABLE 2--LOT SAMPLE. Number of Rolls in Lot or Shipment Number of Rolls to be Tikes for Test 50 and under.................. 3 51 to 100.......................... 6 101 to 250........................ 7 251 to 500........................ 10 601 to 700........................ 12 701 to 1000...................... 15 1001 rolls and over. . . ., 2 per cent of shipment rounded off to the next higher integer. 8. Conditioning 8.1 Condition all specimens (without preconditioning) for a period of 4 hr, or until the specimen shows a progressive change in weight of no more than 0.1 per cent after an exposure of 0.5 hr, in an atmosphere having a relative hu midity of 50 2 per cent at 70 dr 2 F (21 dr 1.1 C). 9. Methods of Test 9.1 Width: 9.1.1 Measure the width of the tape on each roll taken for test by the use of a standard steel rule graduated in i^-in. (1 mm in the case of a metric rule) or finer divisions. Make the measurements while the tape lies flat and without tension on a smooth surface. Make five measurements at least 1 ft (30 cm) apart in each roll. 9.1.2 Report the average of the meas urements on all rolls as the width of the lot under test. 9.2 Thickness: 9.2.1 Measure the thickness of the tape as directed in ASTM Method D 1777, for Measuring Thickness of Tex tile Materials.'1 Use a gage having a circular presser foot with a nominal diam eter of 0.375 in. (9.5 mm). The presser foot and moving parts shall be weighted so as to apply a total load of 6 d: 0.1 oz. (170 3 g) equivalent in pressure to 3.4 psi (0.24 kg/cm1) to the specimen. Make ten thickness-measurements on a speci men from each roll taken for test dis tributed approximately uniformly along the specimen. Make no measurement on the selvage edge of the specimen. 9.2.2 Report the average of all meas urements as the average thickness of the lot. 9.3 Weight: 9.3.1 From each roll taken for test, cut a specimen not less than 5 ft (1.5 m) in length and the full width of the tape, measuring the length of the specimen to the nearest 0.1 in. (2.5 mm), using a steel tape or rigid rule. Make sure that the specimen is free from tension, wrinkles, and folds. Weigh the specimen to the nearest 0.01 oz. (0.3 g). Using the average length and weight, calculate the weight in lb/100 ft (kg/100 m). 9.3.2 Report the calculated weight in lb/100 ft as the weight of the tape. 9.4 Fabric Count: 9.4.1 Ends--Determine the total num ber of ends regardless of the width of the tape. 9.4.2 Picks--Determine with the aid of a thread count magnifying glass the number of picks per inch (25.4 mm) over 1 Appears in this publication. 41960 Book of ASTM Standard. Part 24. D 315) th surface. Make five east 1 ft (30 an) apart average of the measls as the width of the he thickness of the in ASTM Method ing Thickness of Tex~e a gage having a with a nominal diam.5 mm). The presser .rts shall be weighted ll load of 6 0.1 oz. ent in pressure to 3.4 > the specimen. Make : remen ts on a speci' taken for test dis:ely uniformly along no measurement on :he specimen, average of all measrage thickness of the oil taken for test, cut than 5 ft (1.5 m) in width of the tape, i of the specimen to .5 mm), using a steel Make sure that the n tension, wrinkles, re specimen to the ). Using the average alculate the weight m). alculated weight in it of the tape. mine the total numof the width of the mine with the aid 'unifying glass the ch (25.4 mm) over ***4ar4$, ptrt 24 Specification for Woven Asbestos Tape (D 315) i.-npth of 3 in. (76 mm) in each of five Terent places along the specimen. :.4.3 Report the average number of per inch observed for all specimens. 5 . scestos Content: Determine the asbestos content j or more specimens from each roll :.-n for test as directed in ASTM A'.ucd D 191S, Test for Asbestos Con.t A Asbestos Textile Materials.2 6 Breaking Strength {Load): .b.l Determine the breaking load, as :rectcd in 9.6.2 and 9.6.3. Use a speciabout 6 in. (150 mm) long and a .ominai page length of 3 in. (75 mm). a CRT--constant rate of traverse ; re tensile testing machine operated at A -- u.5 in. (305 12 mm) per min. If greed upon between the buyer and eder. a CRE--constant rate of elonga tion machine may be used. 9.6.2 Tapes up to and Including 1.5 in. (38 mm) OVc/e^-Make five tests full width in the warp direction using clamps having a nominal width of 2 in. (50 mm). 9.6.3 Tapes orer 1.5 in. Wide--Make five tests in the warp direction. Use clamps with jaw faces at least as wide as the specimen and insert the specimen in the clamps as directed in ASTM Method D 1682, Test for Breaking Load and Elongation of Textile Fabrics (grab method).4 9.6.4 Report the average of the results as the breaking load of the lot tested. 10. Conformance 10.1 If the test results for the lot con form to the requirements for all charac teristics listed in 6.1.1 through 6.1.8 in clusive, the lot shall be considered ac ceptable. 10.2 If the test results for one or more characteristics do not conform to the re quirements, take a new laboratory sam ple from either the original lot sample or a new lot sample. Test the new sample for the characteristic(s) that did not con form to the requirements in the first test and average the results of the first and second samples as if they were one test of double the original number of specimens. If the new average(s) conform(s) to the specified requirements, the lot shall be considered acceptable. 10.3 If the test results obtained as di rected in 10.2 do not conform to the specified requirements, the lot shall be considered unacceptable. NOTE: ASTM Specifications and Methods of Test are subject to con tinual revision. Consult the Society's current "ASTM Standards on Textile Materials" for possible changes in this specification. Tentative Specification for ASBESTOS TEXTILES USED FOR ELECTRICAL INSULATING PURPOSES1 ASTM Designation: D 2100 - 66 T Issued, 1962; Revised, 1966 This Tentative Specification has been approved by the sponsoring commit tee and accepted by the Society in accordance with established procedures, tor use pending adoption as standard. Suggestions tor revisions should be addressed to the Society at 1916 Race St., Philadelphia, Pa. 19103. 1. Scope 1.1 This specification covers asbestos textile materials used for electrical in sulating purposes having a minimum of 80 per cent asbestos fiber, by weight, excluding the weight of other inorganic reinforcing material which may be present. Note 1--Specifications for other asbestos textiles are covered in ASTM Specification D 299 for Asbestos Yams;' Specification D 315. for Woven .Asbestos Tape;' Specification D 375, for Asbestos Roving;* Specification D 1061, for Asbestos Lap;* and Specification D 1571 for Woven Asbestos Cloth* 2. Definitions 2.1 Asbestos Fiber, n.--For purposes of this specification, asbestos fiber is the hydrous magnesium silicate serpentine mineral identified as chrysotile, and having the general empirical formula MgaSbCyuHy. 2.2 For definitions of other terms used in this specification, refer to ASTM Definitions D 123, Terms Relating to Textile Materials. 3. Classification 3.1 Types--The types of asbestos textiles used for electrical insulating pur poses are based on the following mag netic rating: Type II.................... IV.................. VI................... Maximum Magnetic Rating 0.75 2.0 4.0 3.2 Grades--The grades of asbestos textiles used for electrical insulating purposes are based on the percentage of asbestos content by weight as stated in Table 1. 1 1'ndcr the standardization procedure of the Society, this specification is under the jurisdic tion of the ASTM Committee D-13 on Textile Materials, and is the direct responsibility of Subcommittee A-4 on Asbestos and Its Textile Products. " Ap|ir;ir> in tlii- publication 4. Significance of Types and Grades 4.1 The types of asbestos textiles roughly define the electrical character istics of the material. Generally, the higher the magnetic rating, the poorer o conrds on AL -1 formula terms used to ASTM delating to asbestos lating pur ging mag- ifBCtic Rating 75 0 0 asbestos insulating entage of stated in rades textiles baracterdly, the e poorer C2-t$ f Asbestos Textiles for Electrical Insulating (D 2100) electrical insulating properties of the serial. The three types have the fol- in" intended applications: 1.1 Type II is intended for special -.icaii->r.= where the asbestos is of try importance as electrical insula- >cd r<n maunet wire and when used a dielectric. .'.2 '!; ; IV i- intended for use <-r.- ;:;e ..-i.tsto- is of secondary im-.ar.ct as eiectrical insulation or where, - primary -.'ectrical insulation, it is toned in relatively heavy thickness, -t.t.iiv in comoination with other mateir.is of comparably high dielectric -`renirth. as in the construction of heat TABLE 1 -- r, HADES or ASBESTOS TEXTILES t .-ED roi; ELECTRICAL INSULATING 1'IT.rOSES. Grade AsbeMos tcnient. per ccru Underwriters.............. . . . . A............................. A A ................................ . . . AAA................................ . . . AAAA .......................... . . . . SO to So, end So to 90, end 1*0 to 05, excl 95 to 99, exc1 99 to 100, incl and flame-resistant electrical insulating walls over unit conductors of electrical cables. 4.1.3 Type VI is intended for use where the asbestos is of minor importance as a dielectric, as in fillers for heat- and flame-resistant cables, over-all wraps or braids for such cables, and linings for enclosures subject to exposure to elec tric arcs. 4.2 The grade of asbestos textile used is largely dependent on the service tem perature required of the insulation. Specific temperature limits for the vari ous grades cannot be given as this will depend on the textile construction. In general, the higher the asbestos content, the higher the temperature the textile will withstand. Note 2--Where breaking strength retention is important, good serviceability at temperatures up to approximately 1000 F (540 C) can be expected using the higher grades. If breaking strength retention is not important, asbestos textiles may be used in excess of 1500 F (SIS C), depending on the application. 5. Basis of Purchase 5.1 Asbestos textiles used for electrical insulating purposes are normally pur chased on the basis of type and grade. 6. Materials and Manufacture 6.1 Asbestos textiles used for electrical insulating purposes shall be free of foreign matter not normally present in textiles, which may be detrimental to perform ance. 7. Physical Requirements 7.1 In addition to the requirements of this specification, asbestos textiles to be used for electrical insulating purposes shall meet the requirements of the ap propriate ASTM specification for that particular asbestos textile product (see Note 1). 7.2 Asbestos textiles that have been treated with materials to impart certain desirable characteristics, such as mois ture resistance, flame resistance, and im proved electrical insulating properties, shall conform to the requirements of this specification and also to the applicable ASTM specification for that particular asbestos textile, prior to treatment, or after removal of the treating material by appropriate methods. 8. Methods of Test 8.1 Magnetic Rating--Determine the magnetic rating as directed in ASTM Method D 1118, Magnetic Rating of As bestos Used for Electrical Purposes.* 8.2 Asbestos Content--Determine the asbestos content on specimens from each lot or unit taken for test, as directed in o-ts Asbestos Textiles for Electrical Insulating (D 2100) ASTM Method D 1918, Asbestos Con tent of Asbestos Textile Materials.1 9. Certification 9.1 When agreed upon in writing by the purchaser and the seller, a certifica tion shall be made the basis of acceptance of the material. This shall consist of a copy of the manufacturer's test report or a statement by the seller, accompanied by a copy of the test results, that the ma terial has been sampled, tested, and in spected in accordance with the provisions of the specification. Each certification so furnished shall be signed by an author ized agent of the seller or manufacturer. 9.1.2 When the original identity can not be established, certification can be based only on the sampling procedure provided by the applicable specification. (D 2100) ; results, that the mapled, tested, and in:e with the provisions Each certification so lined by an authoricr or manufacturer. ri"inal identity cancertification can be sampling procedure licable specification. Y APPROVED AS AJfERJCAN STANDARD C59.5&-1963 BY AMERICAN STANDARDS ASSOCIATION UDC 621-315.613.2:620.179.1 Standard Method of Test for AGXETIC RATING OF ASBESTOS USED FOR ELECTRICAL PURPOSES1 ASTM Designation: D1118-57 Adopted, 1957 T!;i? Standard of the American Society for Testing and .Materials is issued under :hc fixed desienation L> 11 IS; the number immediately following the designa tion indicates the year of original adoption or. in the case of revision, the year i last revision. A number in parentheses indicates the year of last reapproval. scope 1. This method covers two procedures for determining the magnetic rating of asbestos used for electrical purposes. The free iron and magnetic iron oxide (Fea04) is determined by a magnetic analyzer and is expressed empirically as magnetic rating (MR). Experience has shown that when used for electrical insulation it is desirable that asbestos have a low mag netic rating. The two procedures de scribed in this method are both based on the principle of comparing the electro magnetic effect of an unknown sample of asbestos with the electromagnetic effect of a known standard. Calibrating Standards 2. (a) A magnetic analyzer covering the usual range of magnetic rating (MR) is designed for two sensitivities: one with a full scale deflection equal to an MR of one, and the other with a full scale deflec-. tion equal to an MR of six. The sensi tivity is controlled by a transfer switch incorporated in the apparatus. For the initial calibration, three to five stand ards, differing in value to cover the test range of the scale, shall be used. A cali brating standard with an MR of one con tains 0.1S g. of National Bureau of Stand ards standard sample No. 29a of iron ore magnetite'-' uniformly distributed over the space occupied by a specimen under test (| in. in diameter by 2J in. in length). For preparing calibrating stand ards of different values, the amount of magnetite shall be varied directly with the value of the desired standard (Note). The calibrating standards shall conform to the following requirements: Since the amount of magnetite used in a calibrating standard is not sufficient to fill the space needed for a test specimen, the magnetite shall be thoroughly mixed with an inert material such as zinc oxide so that it will pack firmly in the space provided. The containers for the calibrating standards shall be made of a nonmagnetic and nonmetallic material and have a chamber for the standard mixture with the same di- 1 I'micr the tnmi:irduation procedure of the Society. thi* method is under the jurisdic tion <>i the ASTM Omimittee D-13 on Textile Mareiial.-. and i> the direct responsibility of Subcommittee A-4 on Asbestos and It? Tex tile l`lot{ih Is. ' Standard sample No. 29a is do longer available from the National Bureau ot Stand ards. A new standard magnetite sample suitable (or this test is available from the General Elec tric Co. Mr P O Nicodemus Wire and Cable Dept Lowell Mass.--Ed K-SI Test for Magnetic Rating of Asbestos (D 1118) tensions as the space in the test speci men holder. A convenient container is a wooden tube 1 in. in outside diameter with an inside diameter of f in. and a length of 4J in. with two end plugs } in. in diameter by 1 in. in length. One plug shall be cemented in place before, and the other after, the standard material is packed. The cement used shall be non magnetic. Note.--In setting up the calibrating stand ards it is desirable to have the magnetic rating equivalent to the percentage of magnetic material present in the specimen to be tested. Because of the variation in the permeability of the oxide*, it may not be possible to accomplish this accu rately. amplifier is zero when no specimen is in the coil. Under this condition, a small amount of magnetic material in one sec tion of S will cause a small voltage at the input to the amplifier due to the increased magnetic flux in that section. This voltage is amplified sufficiently by A to be read by Instrument /. It has been found that the readings of I are nearly directly proportional to the magnetic rating up to a magnetic rating of six. i------------- 1 (b) Secondary standards for routine measurements can be made using smaller containers, that will fit in the test speci men holder, and having sufficient mag netite to give a deflection equal to the calibrating standard corresponding to the maximum scale value. One secondary standard is necessary for each scale range. Procedure A Principle of Operation of Apparatus 3. A schematic drawing of the appa ratus for Procedure A is shown in Fig. 1. The apparatus consists of a testing solenoid T having a primary winding M to produce a strong magnetic field, and secondary windings S and B to measure the change of flux caused by the speci men, a class A audio amplifier, A, to in crease the signal sufficiently to operate an indicating instrument I. This appa ratus operates from a 115-v., 60-cycle power supply. The secondary winding 5 is wound in two equal sections and connected so that their voltages oppose each other when the primary winding M is energized. Coil B is used in series with S to balance out any small voltage difference between the two sections, so that the voltage to the T --Test solenoid if--Magnetizing coil 5 --Secondary coils B --Balancing coil C --Test sample --Alternating current source A --Amplifier G --Amplifier gain control I --Indicating instrument Fro. 1.--Schematic Diagram of Apparatus for Procedure A. The primary and secondary windings of the testing solenoid, the amplifier gain, and the indicating instrument sensitivity can be varied as long as the over-all amplification is sufficient to give a fullscale deflection for the standard corre sponding to the maximum scale value. Testing Solenoid 4. The testing solenoid shall have a primary winding of 17 layers of 0.057-in. enameled single cotton covered copper wire (approximately 4200 turns). This coil shall be wound on a compound tube 2\ in. in outside diameter with an inside diameter of 2 in., a length of 18 in., and .o specimen is in ndition, a small terial in one secill voltage at the ' to the increased : section. This ciently by A to /.It has been of / are nearly i the magnetic c rating of six. tf Apparatus for *y windings of '.mplifier gain, ent sensitivity > the over-all o give a fullindard correscale value. shall have a "s of 0.057-in. cred copper 'urns). This nPound tube "h an inside IlST 70E MAGNETIC RATING 07 ASBESTOS (D 1118) ,-r.d flanges 5 in. square by 1 in. in thick ness. Inside of and concentric with the primary winding is the main secondary .inding. This winding shall be in two .ections on a compound tube 2 in. in outside diameter with an inside diameter of 1 in. and a length of 18 in. having two vinding spaces each 3 in. in length with a diameter of 1$ in. located an equal distance from the ends of the tube and 1 j in. apart. Each section shall be wound with one layer of 0.010 in enameled single silk covered copper wire (approximately 220 turns). These coils shall be electri cally connected so that their voltages are opposing each other. A small sliding coil. B, Fig. 1, shall be connected in series with the secondary winding and is used for fine adjustment of the secondary' voltage. This coil shall be made to slide in the end of the secondary winding coil form with provision to lock it in place at any position up to 2 in. inside the form. The winding space for the sliding coil shall be 1 in. in outside diameter with an inside diameter of | in. and a length of J in. The number of turns on this coil is determined during test as follows: Energize the primary coil from a 115-v., 60-cycle source and measure the voltages across the secondary coils. Then connect these coils in series so that their combined voltage is near zero. Then using a more sensitive indicating instrument, remove turns from the stronger section one turn at a time until it is within one turn of being exactly equal to the other section. Then wind the sliding coil with a sufficient number of turns so that the sections are exactly balanced at some point within its limits of motion and un balanced in opposite directions at the extreme positions the sliding coil can take. This final balancing is usually made with the complete analyzer apparatus and the proper balance is indicated when the indicating instrument will show an appreciable deflection with the balance and then decrease to approximately zero and then increase to an approximately equal unbalance as the coil is moved to its other extreme limit. Test Specimen Holder 5. Test specimens shall be placed in a holder to facilitate setting them in and removing them from the testing solenoid. This specimen holder shall be slightly less than 1 in. in diameter so that it will easily slide inside the secondary coil. It shall be made with a handle at one end and a cork at the other end leaving a space J in. in diameter by 2\ in. in length for the test specimen. The handle shall be made with a stop and its length shall be such that the specimen holder is centrally located under the nearest section of the sec ondary winding when the stop is against the solenoid. Amplifier 6. The amplifier shall be a two-stage resistance-coupled class A amplifier, us ing a pentode (type 57) for the first stage and a triode (type 56) for the second stage. The input is transformer coupled with a high secondary-to-primary-tum ratio transformer. The secondary of the input transformer is shunted by a re sistance to change from the high sen sitivity scale to the low sensitivity scale. This shunt circuit is controlled by a switch mounted on the amplifier panel. The amplifier gab is controlled by varybg the screen grid voltage of the type 57 tube with the potentiometer G, Fig. 1. The bdicating bstrument I, bcluded in the amplifier, is a d-c. milliampere meter with a sensitivity of 1 ma. for a full scale deflection. This bstrument is used with a copper oxide bstrument rectifier for use on alternatbg current. It is coupled to a 30-henry choke b the output of the type 56 tube by means of two 2-/d capacitors. Initial Calibration Test tor Magnetic Rating or Asbestos (D 1118) instrument to balance the secondary windings. After this has been done adjust the over-all amplifier gain to give fullscale deflection on the high-sensitivity (MR1) scale, when an MR1 calibrating standard is in the testing solenoid and the gain control G, Fig. 1, is near its mid position. (Before inserting the calibrating standard, balance the secondary voltage to a minimum.) Switch the amplifier to the low sensitivity (MR6) scale, insert the MR6 calibrating standard in the testing solenoid and adjust the shunt on the input transformer to give full-scale deflection with the gain control G at the same position as used in adjusting the first scale. Then recheck these adjust- Then balance the secondary coils with the balancing coil until the reflection on the indicating instrument is a minimum at full sensitivity. Decrease the sensitivity, place the calibrating standard for the range of test desired in the testing solenoid and adjust the amplifier gain control to give a full-scale deflection equal to the magnetic rating of the calibrating standard. Then remove the calibrating standard, place a 10-g. speci men of asbestos in the specimen holder and insert in the solenoid. The indicating instrument will then give the magnetic rating of the specimen. Procedure B Principle of Operation of Apparatus Fio. 2.--Schematic Diagram of Apparatus for Procedure B. ments to make sure the sensitivities are correct before calibrating the scales. Calibrate the scale by adjusting the equipment to give a full-scale deflection for the calibrating standard correspond ing to its maximum value, then substi tute other calibrating standards and re cord the deflection obtained with them. This shall be done on each scale. If de sired, a special scale can then be marked according to these readings to eliminate correcting all subsequent readings made on the analyzer. Procedure 8. After the initial calibration is com pleted, to determine the magnetic rating of a test specimen of asbestos, first ener gize the apparatus and permit it to warm up for a few minutes to become stable. 9. A schematic drawing of the appa ratus for Procedure B is shown in Fig. 2. The apparatus consists of a series-parallel network of two duplicate test coils Ti and Ft, two duplicate capacitors Ci and Ct, a rectifying unit R, and an indicating instrument /. With an a-c. voltage im pressed on the circuit, the current flow is as indicated by the arrows in Fig. 2. Arrows of solid lines indicate the current flow during the positive half cycles, and arrows of dotted lines indicate the current flow during the negative half cycles. A study of this diagram will show that due to the action of the rectifier, capacitor Ci alternately carries the positive current of coil T\ and the negative current of coil T, while capacitor Ct alternately carries the positive current of coil T, and the nega tive current of coil T,. Therefore, if the currents in both coils are equal, a stable condition exists and no current flows in the indicating circuit. If, however, the currents are unequal, a voltage difference will arise between the two capacitors causing a current to flow through the indicating instrument /. Coils 10. The two coils shall be wound on a nonmagnetic and nonconducting coil 1118) ondaiy coils with the the reflection on the nt is a minimum at rease the sensitivity, standard for the red in the testing the amplifier gain full-scale deflection letic rating of the . Then remove the place a 10-g. speci fic specimen holder noid. The indicating give the magnetic m. ure B a of Apparatus iwing of the appa is shown in Fig. 2. s of a series-parallel ate test coils T\ and lacitors C\ and C, and an indicating .n a-c. voltage imt, the current flow : arrows in Fig. 2. ndicate the current v-e half cycles, and ndicate the current ive half cycles. A will show that due tifier, capacitor C\ positive current of e current of coil 7* rnately carries the T, and the nega. Therefore, if the ire equal, a stable "> current flows in If, however, the voltage difference - two capacitors through the i I | ; l i >) *Clndon* clu,8 coil 7 Test for Magnetic Rating of Asbestos (D 1118) firm approximately 6 in. in length with an inside diameter of I to 2 in. and shall nave several thousand turns each (Note). They shall be as nearly identical in re sistance and inductance as is practicable. Nets.--In one satisfactory apparatus the coils were layer wound with 10,000 turns of '. 0179 in. enameled copper wire on a spool 6| in. in leneth with an inside diameter of If in. and having end fianges 4 in. in diameter by A in. in thickness. of Fig. 3 (4) corresponding to the sketcl of the rectifier unit in Fig. 2. Indicating Instrument 13. The details of the indicating in strument are shown in Fig. 4. This shall consist of a portable galvanometer G, a resistance network for adjusting the over-all sensitivity and for changing the scale range, and a capacitor for by-pass ing any alternating current that may be present. The galvanometer shall have the following characteristics: o b' Fig. 3.--Schematic Diagram of Rectifiers and Connections for Procedure B. ! v/ =c soon ! m-732-L _2-25 rv_____ p bill! ?C00/\ Irt-iOOOA i'/i W' vj^vjvi nToViTrjir------------z--* cz Fig. 4.--Schematic Diagram of Indicating Instrument for Procedure B. Capacitors 11. The capacitors shall be of high quality and have equal reactances (Note). Non.--In one satisfactory apparatus the capacitors were 10-*f. pyranol capacitors insu lated for 330 v., a-c. Rectifying Unit 12. The rectifier shall be made from two conventional full wave copper oxide rectifiers as shown in Fig. 3. Fig. 3 (a) is the conventional full wave rectifier with the d-c. terminals marked ``4-" and "--" and the a-c. terminals marked Fig. 3 (4) shows the connections to be made between two conventional rectifiers to give the desired rectifying unit for this apparatus. Fig. 3 (c) is a simplified sketch Galvanometer resistance, ohms............. 50 Period, sec.................................................... 3 Sensitivity, m amp. per 1-mm. scale division....................................................... 0.040 Extreme critical damping resistance, ohms......................................................... 700 Scale length, mm.......................................... 100 The resistance network shall be made up of stable resistors having low-tempera ture coefficients. The values of these re sistances are approximate as final adjust ment must be made for the particular equipment being used. The capacitor shall be a 50-v. electrolytic capacitor. Test Specimen Holder 14. The test specimen holder shall con sist of a wooden tube 1 in. in outside diameter with an inside diameter of f in. and a length of 4f in. and with two wooden stoppers that extend } in. into each end of the tube. Initial Calibration 15. (o) With this apparatus the balance is greatly affected by the proximity of any magnetic material, as such material changes the inductance of the coils. For this reason magnetic materials should not be used except those that are unavoidable and whose effect can be balanced out, such as the capacitors and the assembly bolts through the rectifier. If these parts are magnetic, the coils shall be mounted with their axes horizontal and parallel, with the capacitors and rectifiers located midway between them. There shall be at Test for Magnetic Rating or Asbestos (D 1118) least 3 in. between the sides of the coils If desired, a smaller variable resistance and the capacitors. A simple balancing can be placed in series with R4 to give arrangement consists of a nonmetallic fine adjustment of the sensitivity. Throw plug, capable of fitting tightly into the the sensitivity switch to the MR6 posi end of one of the coils, with a magnetic tion and place an MR6 calibrating machine screw through its center. The standard in the test coil. Adjust RJ center of the plug should be drilled and keeping the sum of RJ + R2 =* 700 tapped so that the machine screw can be ohms, until a 60-mm. deflection is ob screwed in or out of the coil. A locking tained on the galvanometer. If calibrat nut should be used to hold this screw in ing standards of other MR values are place after balance has been obtained. available, other points on the scale can The length and size of this screw can be be checked and a correction curve ob determined when the procedure described tained, although the deflections are in Paragraph (b) is performed. nearly directly proportional to the MR (A) For the initial balance, the sen values over the range of values used in sitivity of the indicating instrument must this apparatus. be greatly reduced. This can be done by connecting a variable resistance of ap proximately 0 to 100 ohms across the instrument connections to the capacitors. Set the resistor at 0, shorting out the instrument, energize the circuit with a 115-v., 60-cycle supply, and then in crease the resistance slightly until a few millimeters deflection is obtained on the galvanometer. It will then be found that bringing a magnetic screw near the end of one of the coils will cause the galvan ometer deflection to decrease to zero and then reverse as the screw is pushed fur ther into the coil. This indicates that the screw is bringing the coils into balance and then unbalancing them in the op posite direction. Then fit the plug into the desired coil and lock, the screw in the position for zero balance. Increase Procedure 16. Tum the sensitivity switch to the MR6 position, Fig. 4, and energize the apparatus with a 115-v., 60-cycle supply. Balance the apparatus by adjusting the balance screw to bring the galvanometer deflection to zero. Throw the sensitivity switch to the MR1 position, Fig. 4, and rebalance the apparatus, locking the balancing screw in place. Place the MR1 calibrating standard in the test coil and adjust the sensitivity to give a galvanometer deflection equivalent to an MR of one. Insert the 10-g. test speci men of asbestos in the test coil and read the resulting deflection of the galvan ometer. If the deflection is off the scale, throw the sensitivity switch to the MR6 position and read the deflection. the shunt across the instrument and Note.--The procedure here described is ap adjust the balancing screw to maintain plicable only under those conditions wherein the balance until the coils are balanced with the resistance at its highest value. Remove the resistance and readjust the balance. The instrument resistances may now be adjusted to give the desired scale the magnetic particles being tested exhibit no directional properties or when the particle dis tribution is such as to give the ultimate in random orientation. The magnetic particles present in chrysotile asbestos, however, are most frequently needle-like or pseudo-fibrous sensitivities. Place an MR1 calibrating standard in the test coil, throw the sensitivity switch to the MR1 position, and vary R4 to give 100-mm. deflection. and as such exhibit directional properties with regard to magnetic permeability. Therefore, there must be an understanding as to the extent of the fibrous characteristics and the grain t" distribution of the magnetic particles present in ) iable resistance mh R4 to give isitivity. Throw the MR6 posiR6 calibrating Dil. Adjust R1 -r R2 = 700 eflection is obter. If calibrat>IR values are i the scale can tion curve obJeflections are lal to the MR values used in switch to the d energize the 1-cyde supply. adjusting the galvanometer the sensitivity jn, Fig. 4, and , locking the ^lace the MR1 the test coil ty to give a uivalent to an >-g. test sped: coil and read f the galvan% off the scale, h to the MR6 :tion. described it aplitions wherein ited exhibit no be panicle dis- r-t ultimate in cede particles however, are pseudo-fibrous ' roperties with v Therefore, '* "> 'be extent 'be min sire ** present in Test tor Magnetic Rating of Asbestos (D 1118) the sample under test if a proper evaluation of the resulting magnetic rating is to be truly fac tual. In view of the fibrous characteristics of the magnetic particles and the resultant directional magnetic properties, the method of sample preparation and the placement of the sample in the sample holder must be carefully pursued in an endeavor to obtain a test specimen that will exhibit a maximum in random orientation. Calculation 17. The magnetic rating of the test specimen is proportional to the de flection, calculated as follows: MR for the MR1 scale deflection 100 X 1 MR for the MR6 scale deflection X6 60 NOTE: ASTM Specifications and Methods of Test are subject to con tinual revision. Consult the Society's current "ASTM Standards on Textile Materials" for possible changes in this specification. APPROVED A3 AMERICAN STANDARD BY AMERICAN STANDARDS ASSOCIATION ASA NO.: L14.41-19S3 UDC 677.67 .-677.51 .-620.1 NOTE: ASTM Specifications and Methods of Test are subject to con tinual revision. Consult the Society's current "ASTM Standards on Textile Materials" for possible changes in this specification. Standard Methods of TESTING ASBESTOS TUBULAR SLEEVING*1 ASTM Designation: D 628-52 Adopted, 1944; Revised, 1952 This Standard of the American Society for Testing and Materials is issued under the fixed designation D 62S; the final number indicates the year of orig inal adoption as standard or, in the case of revision, the year of last revision. Note.--Section 5 was revised and Section 6 was added editorially in June, 1962. Scope 1. These methods of testing apply to woven and braided asbestos tubular sleeving. Sampling 2. Asbestos tubular sleeving shall be sampled in accordance with Section 10 of the Methods of Testing and Toler ances for Tubular Sleeving and Braids (ASTM Designation: D 354).- Test Condition 3. All test specimens shall be condi tioned to moisture equilibrium in a standard atmosphere having a relative humidity of 50 per cent at 70 F (21 C). A tolerance of 2 per cent is permitted in relative humidity and 2 F (1.1 C) in temperature. . 1 Under the standardization procedure of the Society, these methods are under the jurisdic tion of the ASTM Committee D-13 on Textile Materials, and are the direct responsibility of Subcommittee A-4 on Asbestos and Its Textile Products. 1 I960 Book of ASTM Standardt, Part 24. Note.--For purpose of tests, it is recognized that specimens reach moisture equilibrium after exposure for at least 4 hr at the above specified relative humidity and temperature. Physical Properties 4. Determine the weight, wall thick ness, inside diameter, carriers, ends per bobbin, yarn number, and imperfections in accordance with Sections 11 to 17, inclusive, of Methods D 354. Asbestos Content 5. Determine the asbestos content in accordance with the Method of Test for Asbestos Content of Asbestos Textile Materials (ASTM Designation^ 1918).3 Electrical Properties 6. Asbestos sleeving used for electrical insulation shall conform to the Specifi cation for Asbestos Textiles Used for Electrical Insulating Purposes (ASTM Designation: D 2100).3 3 Appears in this publication. 24-J* X VED AS STANDARD 3ARDS ASSOCIATION : LU.41-I9U ject to conmdards on ition. XG1 :s issued xr of orig: revision. d --Sts, it is recognized ure equilibrium after : the above specified erature. eight, wall thickcarriers, ends per md imperfections ctions 11 to 17, D 354. >estos content in ethod of Test for Asbestos Textile rnation.D 1918).3 ;scd for electrical 1 to the Specifitrxtiles Used for urposes (ASTM un. *-3* x NOTE: ASTM Specifications and Methods of Test are subject to con tinual revision. Consult the Society's current "ASTM Standards on Textile Materials" for possible changes in this specification. Standard Method of Test for HEAT AGING OF ASBESTOS TEXTILES' ASTM Designation: D 1573 - 61 Adopted, 1961 This Standard of the American Society for Testing and Materials is issued under the fixed designation D 1573; the number immediately following the designa tion indicates the year of original adoption or, in the case of revision, the year of last revision. A number in parentheses indicates the year of last reapproval. Scope 1. (a) This method of test is intended for use in the evaluation of asbestos textiles with regard to (/) quality and (2) elevated temperature serviceability characteristics. Since asbestos textiles are usually composed of blends of as bestos with cotton, the latter being present in amounts up to 25 per cent, temperatures above 300 F will pro mote the degradation of the cotton con tent and will reduce the structural rein forcement derived therefrom. In the higher grade asbestos textiles, wherein little or no cotton is used and in which the longer asbestos fibers are necessary if a satisfactory yam is to be produced, the degradation in strength resulting from heat-aging up to 1000 F is low. In the case of the lower grade asbestos textiles, however, wherein amounts from 15 to 25 per cent cotton are incorporated, asbestos fibers having shorter lengths 1 Under the standardization procedure of the Society, this method is under the jurisdiction of the ASTM Committee D-13 on Textile Materials, and is the direct responsiblity of Sub committee A-4 on Asbestos and Its Textile Products. may be utilized. Under the relatively low service temperatures to which such materials may be subjected, neither the cotton nor the cloth properties are greatly affected. However, the strengthimparting influence of the cotton is reduced at elevated temperatures and the entwining properties of the shorter asbestos fibers primarily serve to estab lish the resultant tensile strength and other physical properties of the textile. In view of this, elevated temperature tests may serve to indicate the asbestos fiber grade or quality which may be used in a textile construction. (6) Another use and perhaps more practical application for the information to be derived from elevated temperature studies is the revelation of the ability of a subject textile to withstand known elevated temperature service conditions. It will be appreciated that temperature alone may not be the only degratory influence in the destruction of such materials; however, under normal op erating conditions, high temperatures are usually the dominating factors in such degradation. The results obtained through such investigations therefore -u Test foe Heat Aging of Asbestos Textiles (D 1573) may be interpreted in terms of elevated temperature variations no greater than temperature serviceability. prescribed in Paragraph (a). Standard Test Oven 2. (a) The oven shall be electrically heated and have the necessary controls to maintain temperatures to within 3 C (5.4 F) at any designated testing tem perature up to 800 F and shall have determinable and controllable air circu lation. The air circulation provisions shall be capable of delivering between 100 and 200 cu ft per min continuously to the oven during the testing period. (b) The minimum inside dimensions of the oven shall be 18 by 18 by 18 in., and it shall be provided with two hard ware cloth trays, f in. mesh, 18 by 18 in. upon which the test specimens may be deployed. Pretest Condition of Oven `3. (a) When starting a test, the oven temperature controls shall be set at the desired test temperature at the beginning of the heating-up period. The tempera ture indicating device shall be a chromelalumel thermocouple, or its equivalent, coupled with an accurate potentiometer capable of being calibrated and adjusted to compensate for room temperature and cold junction differentials. The oven temperatures shall be determined by placing the junction of the thermocouple on a sample of cloth supported on the upper hardware cloth tray which will be located not less than 6 in. from the top of the oven nor less than 6 in. above the next lower tray. (6) Air circulation shall be maintained continually from the beginning of the heating period throughout the test cycle. The initial heating-up period, during which no test specimens shall be in the oven, shall be maintained for a minimum of 2 hr or until such a time as the oven conditions have attained the degree of stability that will assure Method of Test Time and Temperature for Test 4. (a) All cloths shall be tested for a period of 2 hr. (5) The temperature for testing shall be dependent upon the grade of the material under investigation, as follows: Commercial Grade........................................ 400 F Underwriter's Grade..................................... 400 F Grade A........................................................... 600 F Grade AA........................................................ 600 F Grade AAA ................................................... 800 F Grade AAAA ................................................ 800 F Deployment of Test Samples in Oven 5. Following the attainment of stabilized conditions, specimens of the samples under test shall be individually positioned on the wire mesh trays. There shall be not less than 6 in. separating the two trays as placed in the oven and not more than 6 in. between the top tray and the top of the oven or between the bot tom tray and the bottom of the oven. With a hearth size 18 by 18 by 18 in., the individual trays will be 18 by 18 in. and on each may be positioned 12 individual grab test specimens. The placements shall be made as quickly as possible so that the oven door will remain open for a minimum length of time in order that the oven temperature may not drop markedly below the testing temperature. Procedure 6. (a) Immediately upon closing the oven door begin the test period and continue the test for a predetermined time. (b) Upon completion of the test period, remove the specimens from the oven and permit them to condition at room temperature for 35 db 5 min. Following this conditioning period, test the speci mens for tensile strength by a method I greater than 5T Test tested lor a testing shall rade of the 1, as follows: ........... 400 F ............. 400 F ............. 600 F ........... 600 F ........... 800 F ............. 800 F s in Oven imnent of r.ens of the individually trays. There parating the ven and not top tray and een the bot)f the oven. S by 18 in.. 18 by 18 in. sitioned 12 imens. The s quickly as i door will n length of temperature v the testing closing the i*nod and '''"mined P"iod, ' r,v'n and *' r 'otn ; '`wing ' 'Ku. * ^"hod u, Test foe Heat Aging of Asbestos Textiles (D 1573) agreed upon by the purchaser and the seller. It is to be understood that tensile strength values (Note) and tensile strength retention values must be established on the basis of cloth con structions, as well as grade, and should be considered individually. Note.--The determination of actual strength values and the decision as to whether such values of tensile strength shall be in terms of pounds break by the grab method or in terms of the percentage strength retention based on the grab test breaks are matters that can best be determined on the basis of the ultimate use to which such information is to be applied. tt-JS X APPROVED AS AMERICAN STANDARD LM.141-1963 BY AMERICAN STANDARDS ASSOCIATION UDC 677-51:620.16siSIJ.676 Tentative Method of Test for ASBESTOS CONTENT OF ASBESTOS TEXTILE MATERIALS1 ASTM Designation: D 1918 - 62 T Issued, 1962 This Tentative Method has been approved by the sponsoring committee and accepted by the Society in accordance with established procedures, for use pending adoption as standard. Suggestions for revisions should be addressed to the Society at 1916 Race St., Philadelphia 3, Pa. Scope Summary of Method 1. (a) This method covers a procedure for determining the asbestos content of untreated chrysotile asbestos textile materials which are usually blends of asbestos and organic fibers. This method is applicable to treated asbestos textile jnaterials only if the treatment can be completely removed, prior to testing, by appropriate methods, such as boiling in water or solvent extraction. (b) This test is limited to those asbes tos textile materials where asbestos is the only inorganic fiber present, or where any other inorganic fiber, such as continuous filament glass yams used as reinforcement, can be removed prior to testing. (c) If carbonates are present in the asbestos they shall be determined separately, and a corresponding correc tion shall be made to the loss on ignition before the asbestos content is calculated. 1 Under the standardization procedure of the Society, this method is under the jurisdiction of the ASTM Committee D-13 on Textile Ma terials, and is the direct responsibility of Sub committee A-4 on Asbestos and Its Textile Products. . 2. (a) If carbonates are not present, a 5-g sample, dried to constant w'eight, is heated to 800 to 810 C (1470 to 1490 F) for 1 hr and the loss in weight is deter mined. The weight of the ignited sample divided by 0.86 is the weight of asbestos fiber originally present in the sample. This weight divided by the original sample weight is the asbestos content calculated as a percentage. (6) If carbonates are present in the asbestos, the weight of carbon dioxide (COi) is determined by the Knorr alkalimeter. The asbestos content is de termined as described in Paragraph (a), but the grams of CO: from a 1-g sample as determined in Section 9 must be sub tracted from the factor 0.86 in calcu lating the results. Definitions 3. (a) Standard Atmosphere for Test ing Asbestos Textiles, n.--Air maintained at a relative humidity of 50 2 per cent and at a temperature of 70 2 F (21 db 1.1 C). (f>) For definitions of other terms used in this method, see Definitions of Terms 14.141-1963 ASSOCIATION .676 ERIALS1 Asbestos Content of Asbestos Textile Materials (D 1918) c t present, a ;t weight, is ) to 1490 F) ;ht is deter'.ited sample : of asbestos the sample. r.he original tos content sent in the bon dioxide the Knorr 'ntent is deragraph (a), i 1-g sample nust be sub56 in calcu- re for Teslr maintained 2 per cent 70 i 2F r terms used >ns of Terms Significance 4. The asbestos content of asbestos textile materials is of major significance, as this determines the grade of the textile, which in turn indicates the approximate serviceability temperature for such ma terials. Apparatus 5. (a) Knorr Alkalimeter, as described in the Appendix and shown in Figs. 1 and 2 for determining carbonates. (b) Oven, capable of being held at a temperature between 800 to 810 C (1407 to 1490 F). Fig. 2.--Absorption Tube for Carbon Di oxide Determination. Relating to Textile Materials (ASTM Designation: D 123). Test Specimens 6. The number of test specimens shall be as specified in the applicable ASTM specification for the material being tested. If the asbestos textile material has been reinforced with continuous filament glass yams, the insertion shall be removed before making the determination. Conditioning 7. Bring all test specimens to moisture equilibrium for testing in the standard atmosphere for testing asbestos textiles. Asbestos Content or Asbestos Textile Materials (D 191S) Procedure for Preliminary Test for Carbonates in Asbestos 8. (a) Determine if heat decomposable carbonates are present in the asbestos by running the qualitative test described in Paragraph (5). (b) Place an approximately 0.5-g sam ple in a test tube (a 30 by 150-mm size is convenient) and wet well with 10 ml of distilled water by stirring and tamping with a glass rod, so that no air bubbles are visible in the wet sample. Add 5 ml of concentrated hydrochloric acid (HC1, sp gr 1.19) and again stir and tamp gently with a glass rod, taking care not to introduce any air bubbles. Warm slightly. The formation of gas bubbles on the surface of the submerged asbestos sample is a positive indication that carbonates are present, in which case the amount of CO: liberated by the carbonates must be determined by the method given in Section 9. If carbonates are not present, follow the procedure described in Section 10. Procedure for C02 Liberated by Carbon ates in Asbestos 9. (a) Check the Knorr alkalimeter (Fig. 1) to ensure freedom from leaks. Aspirate a current of air through the system at the rate of about two bubbles per minute for a period of 10 min. Stop the air current and remove the absorp tion tubes. Place the absorption tube G in the balance case and allow it to stand for several minutes. When ready for weighing, open the stopcocks momen tarily and close. Weigh and repeat the above procedure. The second weight should agree with the first to within 0.0005 g. If it does not, repeat this process until the two successive weigh ings agree. When a constant weight is reached, replace the absorption tube in the gas train. (4) Transfer about 1 g of the sample. weighed to the nearest 0.001 g, to the distillation flask. Wash down any ad hering particles on the inside neck of the flask with distilled water. Add enough distilled water to the flask so that when the apparatus is reconnected the tip of the dropping funnel will be submerged about 5 to 10 mm. Place 50 ml of HC1 (1:1) in the dropping funnel and replace the guard gas-absorption tube at the top of the funnel. Start the flow of water in the condenser and open all the stop cocks, except the one on the dropping funnel. Turn on the aspirator for medium suction. Adjust the stopcock on the dropping funnel so that the suction will draw the acid slowly into the flask. WTien all the acid is in the flask, fully open the funnel stopcock and pull air through the system at the rate of two or three bubbles per second. After the reaction in the flask has subsided, heat the contents gently to boiling. When steam starts to condense in the condenser, turn off the heat. Continue to draw air through the apparatus for 30 min. Reweigh the absorption tube G as before. The gain in weight represents the COj in the sample. Record as C\. (c) Calculate the weight of COj as follows: where: Cj = grams of C02 from the 1-g sample, Ci = grams gain in weight of the absorption tube G, and 5 = grams of sample used. (<f) Repeat the procedure on another 1-g portion of the sample and calculate the average value of C*. The weight of the absorption tube G after the first determination may be used as the starting point for the second determina tion without repeating the initial process of obtaining constant weight. *-n 19 IS) 0.001 g, to the down any adiide neck of the r. Add enough k so that when cted the tip of be submerged . 50 ml of HC1 r.el and replace n tube at the e dow of water n all the stop: the dropping tor for medium pcock on the he suction will r.e dask. When . fully open the dr through the r three bubbles .'action in the the contents 'team starts to r, turn off the . air through 1. Reweigh the fore. The gain e COi in the ht of CO> as he 1-g sample, eight of the .nd I :re on another and calculate The weight of ifter the first used as the nd determinainitial process ht. $-7X Asbestos Content of Asbestos Textile Materials (D1918) Procedure for Asbestos Content by Weight Loss 10.(a) Weigh two specimens, not less than 5 g, each representative of each lot or unit sampled. Place the specimens in crucibles which have been previously heated to 800 to 810 C (1470 to 1490 F) for 1 hr, cooled in a desiccator and weighed to the nearest 0.001 g. Dry the specimens to constant weight at 105 to 110 C (220 to 230 F) and record the weight to the nearest 0.001 g. Subtract the weight of the crucible to obtain the oven-dry weight of the specimen. (b) Place the crucibles containing the specimens in tne oven and heat for not less than 1 hr at 800 to 810 C (1470 to 1490 F). Remove the specimens from the furnace, and cool in a desiccator to room temperature. Weigh and subtract the weight of the crucible to obtain the weight of the ignited asbestos. Record as A. Calculations 11. (a) When carbonates are not present, calculate the asbestos content as follows: A 0.86 _ Asbestos, per cent * --------- ;----------r X 100 weight of sample even if the preliminary test for carbonates is negative, and if CO> is present the necessary corrections shall be made. (b) When carbonates are present, calculate the asbestos content as follows: A Asbestos, per cent -- ------ -------- -- X 100 weight of sample where: Ci -- grams of CO from the 1-g sample as determined in Section 9. (c) To calculate the total inorganic content of asbestos textile materials containing continuous filament glass yams, which were removed prior to test, add the weight of the glass yam re moved from the sample to the numerator and denominator of the equation given in Paragraph (a) or (b). Note 2.--Where a textile contains asbestos and other inorganic fiber, it may be agreed between the manufacturer and the purchaser that the grade of the textile may be considered as the total amount of inorganic fiber present in the textile, but in all cases the asbestos content shall exceed the amount of other in organic fiber present. Report 12. Report the average asbestos con tent of all specimens tested. where: A -- weight of the sample after igni tion, and 0.86 = water of crystallization factor.' Note 1.--If the asbestos content as de termined by the ignition method is lower than expected, the procedure described in Section 9 for determining the amount of COj liberated by carbonates in asbestos may be followed ' The factor 0.86 ia baaed upon a measured average of 14 per cent water of crystallization in chrysotile asbestos. The asbestos content will be in error to the extent that the weight loss of the asbestos differs from the 14 per cent average. When the asbestos contains carbonates which decompose on heating, the weight loss from the decomposition of the carbonates will be com bined with the weight loss from the ignition of the cotton, and an excessive cotton content will be indicated. This may result in an' erroneous classification of the material to a lower grade. NOTE: ASTM Specifications and Methods of Test are subject to con tinual revision. Consult the Society's current "ASTM Standards on Textile Materials" for possible changes in this specification. *-n Asbestos Content or Asbestos Textile Materials (D 1918) APPENDIX Description of Apparatus Al. Knorr Alkalimeter, consisting of the following parts connected as shown in Fig. 1: (a) Gas Washing Bottle, A, containing con centrated H:SO which serves both to indicate the rate of gas flow and to prevent any water /apor entering the system from the atmosphere. (b) Drying Tube or Cylinder, B, filled twothirds full of soda-asbestos absorbent (Ascarite) and one-third full of a drying agent to remove all COi from the air. (e) Knorr Alkalimeter Unit, C, which consists of a dropping funnel, a distillation flask, and a condenser fitted with standard-taper joints to form a unit assembly. (d) Gas Was!;ing Bottle, D, containing a solution of 5 to 10 per cent by weight of AgjSOj in concentrated H:SOt. This serves to absorb any water vapor that escapes from the condenser and to remove any HC1 from the evolved gases. (e) Drying Tube, E, containing CuSO< to ab sorb any H:S generated by the absorption of HCL (f) Drying Tube, F, filled with a suitable drying agent to effect complete drying. (g) Absorption Tube, G, filled two-thirds full of soda-asbestos absorbent (Ascarite) and onethird full of a drying agent, to absorb the COi. (h) Absorption Tube, E, filled with a drying agent and soda-asbestos absorbent (Ascarite) in the reverse direction to prevent CO: from enter ing the system. (i) Trap, /, to prevent back flow of water from the aspirator. (/) Valze or Pinched Tubing, J, to control the rate of air flow pulled through the system by the aspirator. S) .e condenser olved gases. -SO* to ab:ion of HC1. ; a suitable mg. o-thirds full e) and one-b the COi. ith a drying Ascarite) in : from enterjw of water . to control the system i BIX A Glossary of Asbestos Textile Terms Abrasion Resistance--The degree to which a fabric is able to withstand surface wear and rubbing. Asbestos. Ciirysotile--A hydrated silicate of magnesium. Blending--The combining of asbestos fibers of different types, grades or staple length prior to spinning in order to produce a desired and uniform end result. Braid--A narrow textile band formed by plaiting together several strands of asbestos vam. Calendering--A finishing process for fabrics which produces a flat, shiny, smooth surface. It is obtained by passing the cloth through hollow heated calender rolls. Carding--A process of opening and cleaning textile fibers which separates them from each other, lavs them para ".el, makes them into a thin web and condenses them into a continuous, untwisted strand of fibers called a "sliver." This process removes most of the impurities. Clotii, Double--A fabric produced by weaving two cloths, one above the other, on the same loom and binding them together by binder yarns during the weaving operation. Cloth, Listinc--Little used term to designate narrow fabrics or tapes. Cloth, Metallic--A woven fabric of metallic (wire-inserted) asbestos yarn. Cloth, Plain--A woven fabric of plain (non-metallic) asbestos yam. Cloth, Treated--Asbestos cloth impregnated or coated with an organic resin or inorganic compound. Cone, Paper--A conical-shaped core for a yarn package. Cord, Braided--'The product formed by braiding a jacket over a core of yarns or other braids. Cord, Twisted--'The product formed by tightly twisting together two or more plied yarns. Count of Cloth--The number of yarns (or threads) per inch. Cut, Asbestos--Unit of yam measurement used in the asbestos yarn numbering system. It is the number of 100 yard lengths per pound. For single yams, the number of yards per pound is obtained by multiplying the cut number by 100. For plied yams, the number of 97 GLOSSARY--Corn'd yards per pound is obtained by multiplying the cut number by 100 and then dividing bv the number of plies. The latter value is then reduced slightlv for twist contraction by multiplying by a twist contraction factor to give the yards per pound in the plied yarns. End--An individual warp yarn. Fabric Count--The number of warp ends and filling picks per inch in a woven fabric; also called texture, thread count, pick count. Fabric, Slit--A narrow material or tape, without selvage, cut from a wide piece of woven fabric. Felt, Asbestos Dryer--A woven multiple layer fabric serving as a con- vevor belting which carries the moisture-laden paper through the drvcr section of a papermaking machine. Ff.lt, Xon-woven--An asbestos product in sheet formation produced by carding or other fiber orienting process. Fiber, Carded--Asbestos fiber which has been finely divided by carding. Filament--The single individual fiber of indefinite length, such as fila ment ravon, nylon, polyester, etc. Filling--See Weft. Gauce or Cage--The thickness of a woven fabric. Grab Test--Testing of fabrics for strength by a controlled method in which the test is made on a machine, the important features of which are two metal jaws that grip and pull the fabric until it is ruptured. Heiuungbone Twill--A broken twill weave giving a zigzag effect pro duced by alternating the direction of the twill. Lap--A carded assemblage of asbestos fibers in roll form. Pick--An individual filling yam. Plain Weas-e--The most common of the fundamental weaves. Each filling yarn passes successively over and under each warp yarn, alternating each row. Rope, Braided--The product formed by braiding one or more jackets over a core of asbestos rope or wick, by braiding asbestos vam braid over braid, or by plaiting asbestos yam into square cross-section. RorE, Twisted--'The product formed by tightly twisting together two or more strands of asbestos wick. 98 GLOSSARY--Coin'd number by 100 jr value is then ing by a twist e plied yarns. cks per inch in ck count. ge, cut from a rving as a con>er through the Roving. Plain--An assemblage of asbestos or asbestos and other fibei condensed into a strand with no twist as delivered from an asbestc cardincr process. Roving. Reinforced-- As asbestos roving into which a core yarn othc than asbestos has been inserted to increase the roving strength. Selvage of Selvedge--Special varns woven on the extreme outside edg of a woven fabric for the purpose of reinforcement. Sliver. Asbestos--A loose, bulks-, rope-like form, without twist, delivere from a carding process; produced in various weights per yard. Spinning--Process of drawing and twisting fibers together to produc thread or warn. an produced by ded by carding, 'n. such as fila- Staple--Term describing the average length of any fiber. Tape, Metallic--A narrow woven fabric of metallic (wire-inserted) var with selvage edges. Tape. Plain--A narrow woven fabric of plain inon-metallic) yam witi selvage edges. Thread--A treated yarn having high tensile, uniformity and smooth finish Ued method in atures of which il it is ruptured. 'zag effect pro- weaves. Each ich warp yam, ore jackets over >tos yarn braid cross-section. together two or Tube. Paper--A paper cylinder used as a core for a yarn package. j Tubing--Woven, knitted or braided fabrics of cylindrical form. } j Twill--The second basic weave. It has a distinct diagonal line due t( i warp yarns passing over one or more filling yams, then under twe | or more, or vice versa. I Twist--The number of times one inch of yarn is twisted. i Twist, "S"--A yam or cord Twist, "Z"--A vam or cord has "S" twist if the spirals has "Z" twist if the spirals conform in the direction of conform in the direction of slope to the center section slope to the center section of of the letter "s". the letter "z". Warp--The yarn running lengthwise in a woven fabric. Weaving--Process of forming a fabric on a loom by interlacing the warp and filling threads with each other. The fundamental weaves are plain, twill and satin. All other weaves, no matter how intricate, employ' one of these basic weaves in their composition. 99 GLOSSARY--Cont'd Weft--The yarn running crosswise in a woven fabric, or at right angles to the warp threads. Weft is the present English name. Very old term was "woof." American term is "filling" (or yam that fills in). Wick--A soft pliable asbestos textile product formed by loosely twisting several strands of roving or slubbing. Yarn--The product of spinning. Asbestos yarns are continuous strands of spun fibers which are cleaned, drawn and made into yam by a twisting operation on a spinning frame. Yarn, Binder--A warp thread in multiple ply cloths which binds several pieces of cloth together. Yarn. Cabled--A twisted product of multiple ends of plied yam. Yarn, Core--A reinforced asbestos varn in which the reinforcing medium is centered in and covered bv the outer material. Yarn. Cornerinc or Squaring--Those yarns used in braiding to form the corners for square braids. Yarn. Gang Spun--Two or more strands (plain or reinforced) of asbestos rovings combined in a spinning operation. Yarn, Knotless--A continuous length of yarn made from two or more pieces joined together by splicing or a suitable adhesive. Yarn, Metallic--One of more ends of single asbestos yam twisted to gether with one or more strands of fine wire. Yarn, Plain--Yam, either single or plied, which consists of asbestos fiber or asbestos and other fibers. Yarn, Plied--A yarn product produced by twisting together two or more ends of single asbestos yarns. Yarn, Reinforced--Yam. either single or plied, with an insert of yarn other than asbestos to give the product higher tensile strength; some times referred to as inserted yarn. Yarn, Single--A single roving, twisted to give it tensile strength. Yarn, Sized--See Yarn, Treated. Yarn, Stuffer--An extra yarn used to give weight or bulk to a multi-layer fabric. Yarn can be either warp or filling and lies between the face and back of the fabric and does not interweave with the fabric. Yarn, Treated--A yam coated or impregnated with compounds to lay the fibers, increase tensile strength, or impart other properties. 100 "it angles old term twisting `rands of rn bv a s several medium :orm the asbestos or more isted to tos fiber or more of yam h; some- ilti-layer the face >ric. s to lay es. I INDEX Actinolite. 7 Air conductors, flexible. 43 Amosite. 6 textile grades. 22 AnthophvHite. 7 Appliance leads, sleeving for. 52 Asbestos chemical composition of, 7 derivation of word. 1 earls- uses of. 1 effect of temperature on weight, 10 major properties of, 2 table of chemical and mineralogic.il properties. 9 table of physical properties, 8 varieties of, 2 Asbestos textiles elevated temperature serviceability- of, 31 grades. 33 processing of. 24-2S blending. 25 braiding, 28 carding, 25 felting, 28 fiber preparation, 24 forming. 26 inspection and quality control, 2S mixing, 25 spinning, 26 twisting, 26 weaving, 26 radiation stability- of, 33 ASTM Specifications, 60-96 asbestos cloth, 70-73 asbestos content of asbestos textile materials, 92-96 asbestos lap, 60, 61 asbestos roving, 62-64 asbestos tape, 74-77 asbestos textiles used for electrical in sulating purposes, 78-80 asbestos tubular sleeving, 88 asbestos yarns, 65-69 heat aging of asbestos textiles, 89-91 magnetic rating of asbestos used for electrical purposes, 81-87 Cables, sleeving for, 52: wrapping tor, 48 Chrv sotile cobbing of, 19 combustion analysis of. 11 crude fibers. 19 diameter comp, with other fibers. 11 effect of boat on tensile strength, 11 grading of. 19 milled fibers. 16 milling operation, 16 mining ot. 15 origin of. 3 properties of, 3 sources of, 5 surface area comp, with other fibers, 10 tensile strength comp, with other fibers, 10 textile grades, 20 Cloth, asbestos. 42-47 aluminized. 43, metallic i wire-inserted ), 42, 43 plain. (non-metallic), 42 resinated, 43 tables showing grades and construction of typical cloths, 46, 47 textures, 42 treated, 42, 43 weaves, 42 Clothing, asbestos, 42, 43 Clutch facings, 43, 49 Cord, asbestos, 40, 41 braided, 40 metallic (wire-inserted), 40 plain, (non-metallic), 40 table of weights and footages, 41 twisted, 40 Cord, flare signal, 40 Corrugated roofing, sealing, 54 Crocidolite, 6 textile grades, 21 Curtains, industrial, 43 Curtains, lehr, in glass industry, 42 Curtains, safety, for theaters and audi toriums, 42 Belting, conveyor, 42, 49 Blankets, fire-smothering, 42 Boiler expansion door, packing, 55 Brake lining, 43, 49 Draperies, flameproof, 42 Dryer felts, asbestos, 43 Ducts, heating and ventilating, Dust bags, 42, 53 42 101 INDEX-Cont'd Felts, non-woven asbestos, 57 resinated, 31. 57 Fiber, carded asbestos. 53 Fillin':, expansion joint, 56 Filter medium, 5S Firewall seals, 43 Friction materials, 43. 49 Furnace doors, sealing. 54, 55 Furnace hoods, industrial. 42 Gas generator doors, sealing, 55 Gaskets, 40, 43, 45, 55 Insulation boiler, jacket for, 42 bus bar, 53 cable, 36, 4S. 52. 57 diesel exhaust line. 55 fixture wire, 34 glass handling tools. 40 heater cord. 34, 36 heating elements, 36 motor winding, 4S pipe, jacket for, 42 resistance wire, 40, 41 Ironing board cov ers, 42 Lap, asbestos, 34, 35 Laundry flat work ironers, covers for, 42 Magnetic Rating, 78-80 method of test for, 81-87 Manhole covers, gasketing for, 55 Missile components, 43, 57 Noise quieting, 42 Nuclear reactors, shields for, 42 Ovens, industrial, sealing, 54 Packings, 43, 48 emergency, 54 groove, 55 high temperature, 54. 55 steam and,hot water valve, 54 stuffing box, 58 valve stem, 40 Pads, stress-relieving, in welding opera tions, 48 Pincers, glassware, covering for, 52 Plastics, reinforcement for, 57 Quebec Standard Screen Test, 19 Retorts, caulking of, 54 Rocket components, 32, 43, 57 Rope, asbestos, 55, 56 braided, 55 table of weights and footages, 56 twisted, 55 Roving, Asbestos, 36, 37 plain, 36 reinforced (core or inserted), 36 table of cut numbers with nominal yds. per lb. and permissible variations, 63 Sleeving, tubular, see Tubing, asbestos Steam hose, braided wall for, 40 Tape, asbestos, 48-51 metallic (wire-inserted), 49; table of thicknesses, widths, footages, 50 plain, (non-metallic), 48; table of thicknesses, widths, footages, 51 treated, 48 Thermocouples, covering for lead wires of, 52 Thread, asbestos, 41 metallic (wire-inserted), 41 plain, (non-metallic), 41 Tongs, glassware, covering for, 52 Tremolite, 7 Tubing, asbestos, 52, 53 braided, 52 treated, 52 woven, 52, 53 Wall covering, flameproof, 43 Welding booths, shields for, 42 Wick, asbestos, 54 Wire wiping pads, 58; wick, 54 Yarn, asbestos, 38, 39 metallic (wire-inserted), 38, 39 plain, (non-metallic), 38 plied, 39 reinforced, 39 single, 39 table of cut numbers of plain single yams with nominal yds. per lb. and permissible variations, 66 treated, 39 102 \ < Compliments oj RAYBESTOS-MANHATTAN, INC. , Asbestos Textile Division Manheim, Pa. No. Charleston, S. C. Additional copies oj this handbook available on request ' -v v, _ ^^^ _ . .-- - - ,* - V-`,1. . J. VV* \ V.;:X *' >.' *.-'T'h t7irfjC3 - 7'rc?i- .. r: -? v. .-iMitesS 'vt.T.V*1--V* 1 . jjSiy s r . w . . -. ->>, , . ' *` , . - - t* . - * ?** **;** tJ^SfcSfiS