Document nNr2K7qZOowO4OjnD7yg0nZem
Johns-Manville Research Center
Report No. 425-649 Date October 21, 1957
Title: EVALUATION CP ASBESTOS FIBEHS USSR IN TRANSITS PIPE
i
sssfisshtiaij
SGMHARI
The purpose of this Investigation was to determine the drainage-filtration time for asbestos fibers and the relative unit strengths and densities of sag cakes made with these asbestos fibers currently used in the manufacture of Transits pipe* For a given percentage of fiber in the furnish, a given consistency, and' a constant forming pressure, the relative strengths of the sag cakes and the drainage-filtration times for the fibers are given below:
Relative Strengths - C&G3 = 100$
Relative Drainage Filtration Rates CS& = 100$
Tiber
Percent of Obit Strength Maximum
C-K53 1 4T28
Cleaned 6020
Normandie 4T
5R21 6020 Mnnro 4T Rhodesian S Scrap
4260 4050
4050 3560 3520 3450 3330 3200 1740
100 95*3
95.3 83.5 62.8 81*1 78.3 75.3 40.8
Fiber
Scrap C403
Drainage Percent of Maximum Filtration 1/frrainage
32 285.0 91 100.0
Normandie 4T Mnnro 4I Rhodesian S
4T28 Cleaned 62)20
5R21 62)20
115 120
215 350 400 570 635
79.0 :
- 75.8 42.4 26.0 22.7 16.0 14.4
Relative Strengths of Blue Fibers * MS Blue = 100$
25$ Fiber in Furnish
Fiber
Uhit Strength Dai
Percent of Maximum Strength\
MS Blue Australian Blue
3700 3500
100 94.5
Norca Blue
2530
68.4
Relative Drainage Filtration Hates of Blue Fibers - MS Blue = 100$
6 gm Fiber per 2110 cc Water
Drainage Percent of Maximum
Fiber
Filtration l/brainage Filtration Time
Norca Blue
Australian Blue
MS Blue
62 91
109
176.0 120.0
100.0
................. ^47. DU 31-64
FUe 425
JOHNS-MANVUXE RESEARCH CENTER
Report'No: 425-649 Page Sinn; - Cont'd
The strengths were determined from sag cakes made with fibers obtained from the Manville plant in 1957* The strengths given are the average value of ten samples for each condition, and the dry ingredients for each group of samples were "batch" mixed in the Readco Mixer. A randomized procedure was followed in making all samples. The results on the blue fibers were separated from those of the other fibers because of the "bulking" characteristics of the blue fibers and the considerably lower densities and effect on strength that result.
The values obtained in this investigation agree in general with those presented in Task Force Report No. 12 and No* 83* Particular note should be made of the low strength of Norca Blue fiber, and it is suggested that the use of this fiber be curtailed if a sufficient supply of MS Blue or Australian Blue fiber is available. The values presented in this report should in no way be construed as representing absolute values; rather, they indicate the relative variance that may be expected in using these fibers.
Contents: Sunanary, Discussion, Appendices.
mo cc: C. 7. Rassveiler, GHQ (3)
C. F. Hassweiler . Attn: H. S. Allen (0) B. F. Orth, DHQ
To be noted by J. H. Goodwin G. R. R. Wahl, DBQ 1 T. R. Turnbull, DHQ K. J. Whalen, DHQ A. J. Maahs, DHQ S. Collier, GHQ F. T. Petersen, DHQ' J. Wo Miles, Marrero J. La Miller, Waukegan
A. Harris, Watson 4. H. Schilling, Stockton W L. VanDerbeek, Manville J. E. Hesse, Denison R. S. Gardner, Toronto J. D. Iowry, Toronto B. R. Williams (2) (+S) J. A. McKinney
J. Q. Trice G. Snolak File (2)