Marshall laboratory June 30, 195^
PREPARED BY: * R. A, RGBICHADD
LABORATORY EVALDATIOR OF SHERWIH-WILL1AES WATER REDUCIBLE BLACK HAMEL
Introductions
Sherwin-Williams offered this product at Hardwick Stove company, Cleveland, Tennessee, as a replacement for a black japan 1 baking enamel. Customer la .apparently satisfied with the working properties but is .hesitant about using a material that is so radical
in nature. Because of lts'noveltyj Atlanta.Sales asked the labor atory to examine'-a' coated panel. Atlanta was also able to supply us with a sample of wet material for-complete evaluation,
This report, the first formal one,`will include results of tests reported in other correspondence in .addition to the writer's evaluation of the enamel*
Conclusions t
The S-W water reducible black was extremely water sensi
tive, exhibiting poor humidity cabinet, salt spray and water soak resistance. Appearance of the dry film is gritty* However, its selling price, reported to be under $2,50 per gallon, and the fact that it can be reduced with water* introducing solvent savings and probable insurance cost reduction, make it attractive. In addition, this formulation is undoubtedly in the experimental stage and im provements can be expected In the future.
N35495
Experimental Work:
A. Composition
.Bolide. V` h-'' > $
18.3$ (spray viscosity)
Reduction
67$ (3 pts. namel/2 pts. water)
Nitrogen content
1.24$
Viscosity
57" (20 cap)
wt./Gai,
8.49#
Plash Point
Non
0. D. Shreve , in his letter/to Russell Morgan dated
4/5/54,. reported that this enamel was:composed of an alkyd, mela mine, TIP and rosin vehicle. His observations (supported by the writer's examination) indicate that the enamel is truly water
soluble and not an emulsion type. There Is some evidence, however, that the ^educing thinner (water) probably emulsifies*
Appearance and Application?
The enamel has an exceedingly gritty appearance. While a felt strainer removed most of this, the more common mesh types
had very little effect. The panel sent in by Atlanta had the same
poor appearan.ce,
*
Due to the low solids we were unable to obtain more than 0,3 mils film thickness by spray application without sagging. There
for, multiple coats (2 or 3) are required to get 1.0 mils film
thickness. This is further hindered by the slow flash time (3/4 to 1 hour) and the necessity of baking between each coat. Failure to
allow sufficient flash time or to bake causes.severe blistering.
We encountered no difficulty in ignoring the recommended 20 minutes waiting period after reduction before use. A pour, dip and spray were mad immediately after reduction with no noticeable ill effects.
Testing Results1
Air"drying was completely unsatisfactory. The film was tacky for 1-2 weeks and was water soluble' and soft after two. months.
Baking; produced a satisfactory :film. For comparison, 707-6230 was run with the S-W enamel as a control. 707-6230 was
DUP030003697
3~
baked in all cases 30' at 300P. The following charts summarise results (all films are 1.0+ 0.1 mils):
Bake
Pencil Hardness
Black
15` at 250P .
SB
45* at 250^F.
F
5* at 350F..
IB
Recommended baking schedule is reported to be 5* at 350F.
GIOSS Flex.-
S-W BLACK
707-6330
Steel
Bonderlte 100 Steel
Bonderlte 100
79 88 88
95
V. Good
V, Good
V, Good
Fair
Salt Spray
V, Poor
Humidity Cabinet V. Poor
Poor Poor
Good V. Good
7. Good 7. Good
Adhesion
Good
Good
Good
Good
Accelerated weathering test on S~W black revealed fine cheeking, chalking and dulling at 400. hours. ( The control had very slight chalking and dulling. Water soak produced blisters within
a few hours on baked panels. After Immersed portion was dried out, film lost adhesion and became brittle. The control had excellent water soak resistance. Heat resistance (X week at l80eF.} was very good, slightly superior to 707-6230.
A somewhat interesting sidelight was the lack of rusting under the S-W black films subject to the various water tests. In
spite of severe blistering and loss of adhesion, very little rusting appeared beneath the film on the bare steel panels.
General:
Information on test methods and other details are In Note book #5665, starting On Page 140,
Exposure Series #13739 has been prepared on this material.
SALES DEVELOPMENT
RAR/&AW 6/25/54 - R
6/30/54 - T
R. A. RCBICEftUD