TECHNICAL SERVICE REPORT Union Carbide Corporation Metals Division
P.0. Box 579 Niagara Falls, NY 14302
PLAINTIFF'S EXHIBIT
Date:
April 2, 1979
Subject: Author:
Plenum Chamber Airborne Fiber Emissions of Oil-Treated Super Standard 1/8" Pellets Exposed to Ambient Conditions
B. L. Ingalls
Report No. 2272-34
File Ho.
3.6.13.2.4
Oil-treated 1/8 inch super standard grade pellets prepared at King City were evaluated for fiber emission characteristics after exposure to ambient weathering conditions.
Several hundred grams of the oil-wetted pellets (24.5% oil by wt. as received) were subjected to weathering in an open, unheated warehouse for a period of 38 days. Ambient temperatures ranged from sub-zero to 45F. The pellets were weighed periodically and subsequently tested for fiber emission characteristics in a laboratory plenum chamber.
The plenum test involved subjecting 50 gram samples of the pellets to 5 and 15 minutes of vibration in an 8-inch diameter pan, 2 inches high, mounted on a Derrick vibrator enclosed in a 6 ft. chamber. The degree of vibration was controlled at a constant level. Two MSA samplers con-r taining Milliport 0.8 membrane filters were suspended inside near the top of the plenum chamber. The atmosphere in the chamber was monitored continuously at a rate of 2 liters/minute over the 5 and 15 minute periods. The airborne asbestos was counted in accordance with OSHA procedures under Federal Regulation 1910.001 using phase contrast microscopy.
The oil-treated pellets as received from the plant were dark green in color. The pellets appeared to be slightly lighter in color after four days exposure. No significant changes were observed over the following two to three weeks. After approximately three weeks, the pellets light ened in color and ultimately developed the appearance of dry untreated product (refer Figure 1). The amount of oil loss with exposure time is demonstrated in Table I and Figure 2. Approximately 2.5% by weight of the oil evaporated after four days (based on the initial loading). After 38 days, the amount of oil in the pellets had decreased from 24.5 to 18.4%, representing a 25% loss of oil due to evaporation.
X400732
2- -
Plenum test results are summarized in Table II. Control samples were obtained throughout the tests to determine background levels in the chamber. The chamber was vacuumed and wiped with a damp sponge before and after each set of tests. However, residual background fiber averaged ^0.3 f/cc for the controls with a rangeof 0 to 1.0 f/cc. Samples tested after four days exposure averaged 0.6 and 1.4 f/cc for the 5 and 15 minute tests, respectively. Pellets' exposed for 38 days demonstrated average fiber emissions of 1.9 and 4.5 for the 5 and 15 minute plenum tests. The plenum emission characteristics of untreated crushed supervisbestos were also included for the purpose of comparison. Fiber emissions of crushed SVB were roughly 20 times that of the oil-treated pellets exposed for 38 days. The plenum test Is far more rigorous than any conditions anticipated in field application. Furthermore, oil-wetted product would be packaged in a manner to prevent evaporation. The principle concern and objectives of this study relate to product exposed to ambient conditions due to spillage around the hopper and an occasional breakage of bags. As such, it is most unlikely, based on the data, that oil-wetted pellets would significantly raise the air borne fiber emissions. The primary objective of oil treatment is to contain fiber emissions within a TWA of 0.1 f/cc. Emission tests conducted on oil-treated pellets in the field were all well within a 0.1 f/cc TWA. The effects of prolonged exposure on residual material should not significantly alter emissions on the basis of these data. However, an extended field trial should be conducted for confir mation.
/rm Attachments
X400732
FIGURE I Oil-treated 1/8 inch super standard pellets. Material on right as received (24.5% oil by wt.). Material on left - after 38 days exposure (18.4% oil by wt.).
X 400734
C v n A n iv a T in a ^
^
!
TABLE I PERCENT OIL LOSS WITH EXPOSURE TIME*
1/15/79 As Received 1/19/79 After 4 Days Exposure 2/23/79 After 38 Days Exposure
X Oil by Wt.
24.5 23.9 18.4
Based on oven drying *^18 hours at 1058C.
% Oil Loss
2.5 24.9
TABLE II AVERAGE PLENUM TEST RESULTS (FIBERS/CC)*
5 Min. Plenum Test
Control
0.3(0-1.0)**
Oil-Treated 1/8" Pellets After 4 Days Exposure
0.6(0.2-0.8)
Oil-Treated 1/8" Pellets After 38 Days Exposure
1.9(1.5-2.4)
Crushed SVB
35.9(30.5-40.7)
15 Min. Plenum Test
0.2(0.1-0.5)
1.4(0.2-3.3)
4.5(2.2-6.8)
Reference Data - Tables III & IV Range-Fibe rs/c c Too heavily loaded to count.
X400736
TABLE III
PLENUM TEST RESULTS AFTER 4 DAYS EXPOSURE (fibers/cc of air)
Control Oil-Treated 1/8" Pellets Control Oil-Teated 1/8" Pellets Control
Oil-Treated 1/8" Pellets Control Oil Treated 1/8" Pellets Control Oil-Treated 1/8" Pellets
5 Min. Plenum Test
Sample #1
Sample #2
0.3 0.3 0.6 0.8 0.6 0.1 0.2 0.6 0.0 <0.1
-- -' --
--
15 Min. Plenum Test
Sample #1
Sample #2
--
0.6 0.2 0.3 0.2 2.2 3.3 0.0 0.5 0.9 1.1
TABLE IV
PLENUM TEST RESULTS AFTER 38 DAYS EXPOSURE (fibers/cc of air)
Control Oil-Treated 1/8" Pellets Control Oil-Treated 1/8" Pellets
Control Oil-Treated 1/8" Pellets Control Oil-Treated 1/8" Pellets
5 Min. Plenum Test
Sample #1
Sample #2
0.2 0.4 2.1 1.5 0.2 1.0 2.4 1.7
_ -_
--
15 Min. Plenum Test
Sample #1
Sample #2
_
--
0.2 0.2 5.8 6.8 0.2 0.1 2.2 3.3
X4CC737
TABLE V PERCENT OIL LOSS WITH EXPOSURE TIME*
Date
1/15/79 1/16/79 1/17/79 1/18/79 1/19/79 1/26/79 2/20/79 2/23/79
% Oil by Ht.
24.5 24.5 24.5 24.5 24.4 23.9 18.0 17.8
% Oil Loss
. 0.4 2.1 26.1 27.0
*Based on total weight loss measurements.
X400738