Document mqJq67BZXr5OMyXEgZ6KagvqQ

OKOAN IO D)^'KLOPflENlWOW3ftNf<4lrRADE LITERATU I BULLETIN PERMANENLFILE.' PLANE RETARDANT POLYETHYLENE ^^3 development department MONSANTO CHEMICAL COMPANY ORGANIC CHEMICALS DIVISION ST. LOUIS H, MISSOURI TO ASSIST YOU IN THE EVALUATION OP THE ABOVE PRODUCT, WE HAVE OBTAINED THE INEORMATION CON TAINED IN THIS BULLETIN FROM LITERATURE SOURCES AND PRELIMINARY INVESTIGATION IN OUR OWN lABORATORIES, WHILE WE BELIEVE THE INEORMATION Is ACCURATE. Wt ASSUME NO RESPONSIBILITY AND disclaim ANY Liability incurred in Using these data or suggestions, only qUaiihed tecHNIcAI PERSONNEL SHOULD WORK WITH THIS PRODUCT UNTIL SUBSEQUENT STUDIES JUSTIFY ITS USE IN YOUR PROD UCTS OR PROCESSES. OBVIOUSLY NOTHING IN THIS BULLETIN SHOULD BE CONSTRUED AS A RECOMMEN DATION TO USE ANY PRODUCT IN CONFLICT WITH EXISTING PATENtS COVERING ANY MATERIAL OR ITS USE. With the recent requirements for flame retardant plastios, defined by the Underwriter Laboratories, Interest In pro ducing satisfactory compounds'for applianoe applications has substantially Increased. . This teohnioal bulletin presents data on Aroclor Modiiy.edPlame Retardant Polyethylene. It compares the polyethylene, modified with Aroolor 5460, to -polyethylene containing similar amounts of a 70$ ohlorinated paraffin. Aroolor 5460 will produce flame retardant polyethylene added per se at 30jfe"weight or at 20# by weight in combination " with 10?6 Antimony Oxide. These additions improve -Melt Index, slightly reduce Memory, retain Tensile Properties and reduoe compound costs. . At equivalent concentrations, the effept on the physloal properties by Aroclor 5460 are significantly less pronounces than the 70?6 ohlorinated paraffin. Heat stabilities of the Aroolor systems are significantly better than the pararrin modified polyethylene. Aroolor 5460 la a 60# ohlorinated terphenyl. It is oowmer- daily availa. bly at the following pricneasr!s la WiiP ....... *Carload or Truckload *L5C-gL aollronLTcL ontainer Jc'/ik I3n0.'2l5l'//llbb* All prices F.O.B. - Anniston, Alabama P"racked in 500 fibre drums Samples of Aroclor 5460 are readily available standard sample size is onfe pound. 0627432 TOWOLDMON0039999 WATER_PCB-00024468 2 following in Table 1 below are comparative teBt results on combinations of polyethylene with Aroclor 5460, a 70# chlorinated paraffin and Antimony Oxide. The Melt Index and # Memory values were determined using condition E of ASTM 1238-57T except that in all cases 9 grams of material were charged into the cylinder. Tensile properties were determined on miniature specimens with the Instron at a Jaw Bpeed of 10 inches a minute. The burning tests were conducted as followsi Strips of polyethylene, l" x 4" with lines scribed " from each end, are hung in an asbestos cylinder 2-|" in diameter and 511 ' in length. A bunsen flame, 1" high, le used to ignite the specimen. When the,, e flame reaches the first scribed mark, the flame is removed and a stopwatch started. The time to flame out or.to . the second soribed mark is measured. Note (in Table 1, next page) that the 30# modification by Aroolor 5460 has tensile properties superior to the 20# modification by the ohlorinated paraffin. This reduoed effeot on tenBiles at the higher modification is also true when 10# Antimony Oxide is added. git i 062 7433 i ... ^-f TOWOLDMON0040000 WATER_PCB-00024469 , 3- TABLE I Properties of Low Density Polyethylene Modified with Aroclor 5460 and a 70# Chlorinated Paraffin Control Melt # #ElonIndex Memory Kation 1.96 57.2 655 80# poly ethylene 20# Chlor.' Para. 70# poly ethylene . 30# Aroclor 5.9 11,2 70# poly ethylene 30# Ohlor. Para, 10,5 80# poly ethylene 10# Ohlor. Para,,10# Antimony Oxide .- 3.6 70# poly ethylene 20# Aroclor 10# Antimony Oxide 6.2 70# poly ethylene 20# Chlor. Para,, 10# Antimony Oxide 6.4 61.5 51.5 67.6 59.0 52 54 585 647 130 655 650 540 Burn Tensile Yield Rate Self- ExtinEulshlnK 2130 1395 7.1 in/ No min. 1640 1450 0 1850 1320 0 Yes Yes 1175 1195 0 Yes 195 . 1445 0 Yes 1710 1300 0 Yee. 1200 1320 0 Yes O'- ; . 0627*3* TOWOLDMON0040001 WATER_PCB-00024470 -4- In Table II the heat stabilities of variously modified poly ethylene are compared. Note the significant improvement in heat stability when the Aroclor 5460 is the modifying agent. These values are Important to the molder Where the modified polyethylene may be held at high temperatures for an extended period of time. TABLE II Heat Stability of Modified Polyethylene (Air circulating over at 190c) Time (Min.) 0 10 20 4o 60 Control white off-wh. offwh. off-wh. sl.yel. 80# polyethylene 20# Chlor.Para. yl.-tan dk.tan lt.bm, brown dk.bm. 70# polyethylene 30# Aroolor 5460 It.yel. It.yel. It.yel, It.yel, mod.yel, 70# polyethylene 30# Chior. Para, dk.tan lt.bm. brown dk.bm. blaok BO# polyethylene 10# Chlor.Para., 10# Antimony Oxide white white It.tan tan dk.tan 70# polyethylene 20# Aroclor 5460 10# Ahtlmony Oxide white white white . off-wh. It.yel, 70# polyethylene 20# Chlor.Para, 10# Antimony Oxide wh.-tan It.tan tan dk.tan lt.bm 0627*35 TOWOLDMON0040002 WATER_PCB-00024471 -5- Following ih. Table III are the general physical properties of Aboolor 5460, TABLE 111 - AROCLOR 5460 r. PHYSICAL PROPERTIES Form Color Acidity Specific Gravity S5/25C. Pounds per gallon Flash Point* Fire Point* Softening Point Yellow transparent reBin 2.0 NPA 0.07 (mgm KOH per gram) 1.670 13.91 None None 100 - 105.5C. * Cleveland Open Cup RMP/se - 300 10/26/59 0627436 | tow5ldmono64oo(^3 WATER_PCB-00024472