OHIO AGRICULTURAL RESEARCH AND DEVELOPMENT CENTER Wooster, Ohio
MONS 07U09
BARRIER COATINGS TO PREVENT POLYCHLORINATED BIPHENYL (PCB) CONTAMINATION OF SILAGE*
L. B. Willett Department of Dairy Science
Polychlorinated biphenyls or PCB's, also often called by their trade name Aroclors (Monsanto), have been recently in the news as "new" chemical contaminants found in livestock feed and subsequently in meat, eggs, poultry, fish, and milk. The discovery of these compounds has caused considerable concern among those asso ciated with animal agriculture and considerable financial loss to those directly affected by this contaminant.
PCB's are a family of stable chlorinated hydrocarbons which upon analysis may appear quite similar to DDT. They, like all synthetic chlorinated hydrocarbons, are illegal contaminants of human food. PCB's are chemically quite inert and are not broken down by acids, alkalies, or corrosive chemicals. They have a high boil ing point and do not bum readily; they only vaporize. Thus PCB's have the neces sary physical and chemical characteristics for persistence and accumulation in the food chain.
Polychlorinated biphenyls were first described in the scientific literature in 1881 and commercial production was successfully achieved in 1930. Between 1930 and 1969, the USDA listed 55 different industrial or agricultural applications of PCB compounds, many of which represented potential sources of environmental, food, and feedstuff contamination. Some products which have contained PCB's include: elec trical insulating fluids, tires, printing inks, flame-retardant paints and fabrics, carbonless self-duplicating paper, some insecticides, and concrete coatings. Inter estingly enough, PCB's were only discovered as an environmental contaminant in 1966.
A large number of silos in Ohio and neighboring states have been coated to prevent leakage and erosion of the walls with a material containing PCB's. The PCB found in greatest quantities in these coating materials is Aroclor 12S4. This PCB material migrates from the silo coating into the silage. Then it is consumed by and accumulated in the livestock. So the PCB residues can ultimately be deposited in human food products produced by livestock fed the contaminated silage. If the concentration of this residue exceeds the Food and Drug Administration's "adminis trative guideline," the product can no longer be marketed.
The mechanism by which PCB's from Aroclor-containing coatings contaminate the silage, and in turn the livestock, was originally believed to be only mechanical-- caused by flaking off of contaminated chips. It is not uncommon for these chips to contain 5,000 to 10,000 p.p.m. (parts per million) of Aroclor. However, recent work at the University of Kentucky has shown that the Aroclor in the coating mate rials is soluble in silage juices.
The replacement of contaminated silos with new ones would represent a consider able financial loss to dairymen and cattlemen. Therefore, studies are being con-
Appreciation is expressed to the following organizations for their support of
this research. Action! Plastic Inc., Charlotte, Mich.; Ohio Milk Producers Federa tion, Columbus; Ohio Silo Company, booster; Silver Bros., Inc., Wooster; Standard Dry Wall Products, Inc., Miami, Fla.; and United Cooperatives, Inc., Alliance, Ohio.
-28-
MGNS 071210
ducted at the Ohio Agricultural Research and Development Center to determine how ef fective coating materials may be in preventing further PCB contamination of silage. Tlic results of the first trial are presented in this report.
Two lines of investigation were used in this study. A silo which had been previously treated with a coating containing Aroclor 1254 was used as the major structure. The silo was divided with sheets of Masonite into test sections, the walls were wire brushed to remove loose material, and the surfaces were coated with materials (Tabic 1) considered impervious to the PCB in the silo walls. Untreated and wire-brushed test sections were left as controls.
TABLE 1.--Identifications, Principal Components, Principal Solvents, and Test Locations of Barrier Coatings Tested.
Coating Numeral
1
Coating Type
Furfuryl
Principal Component or Resin
Furfuryl alcohol resin
Principal Solvent
Isoprophyl alcohol
Where Tested STTo-----EToH
XX
11 Vinyl
Vinyl resin
Methyl isobutyl ketone
XX
111
Epoxy sealer
Epoxy resin
Xylene
X
IV Epoxy sealer + Epoxy resin
Epoxy topcoat
Xylene
X
V Epoxy sealer + Epoxy resin
Epoxy topcoat
Cellosolve X X
VI .
Water epoxy
Epoxy resin
Water
X
VII
Thermoplastic
Alkyl aeromatic
hydrocarbon
hydrocarbon
Kerosene
X
VIII
Hydraulic cement
Cement
Water
XX
IX
Vinyl sealer
Vinyl resin
+
_ Methyl isobutyl ketone
Vinyl topcoat
Vinyl resin
Methyl isobutyl ketone
XI
Epoxy sealer
Epoxy resin
++
Water epoxy
Epoxy resin
Xylene Water
XX
-29-
MGNS 07U11
The silo was filled to the top of the experimental sections with chopped corn (32* dry matter). Four months later, the spoilage was removed and silage samples were collected at three levels in the silo and at five distances from the silo wall. The samples were analyzed by gas chromatography (with electron capture detector) for Aroclor 1254 in order to determine the effectiveness of the coating materials and to determine the vertical and horizontal distribution of any PCB contamination.
In other studies, concrete silo blocks were painted with a coating which con tained Aroclor 1254. Then the blocks were rccoated with the materials designed to prevent PCB migration. These blocks were scaled in 55-gallon barrels of chopped corn for 4 months. The silage was then sampled at three depths and at three dis tances from the blocks and analyzed for Aroclor 1254.
The results of the tests conducted in the silo are shown in Figure 1. In those tests, all of the coating materials reduced the amount of Aroclor 1254 migrating in to the silage when compared to the untreated control. However, only coatings I and VIII reduced the contamination level to below that of the wire-brushed control sur face. Statistical analyses to determine if the observed differences are significant have not been conducted yet.
The reasons why coatings 1 and VIII provided the best barrier to the PCB arc not thoroughly understood. It is suspected that the solvents used in the other coatings tested (II,V, IX) dissolved more Aroclor from the silo wall than the isoprophyl alcohol and water used as solvents in coatings 1 and VIII, respectively. When Aroclor becomes dissolved by the solvent of a new coating, it can then become
a component of the new surface.
In all test and control sections, the majority of the contamination was detected in the silage within 30 cm. (1 ft.) of the silo wall. Likewise, the concentration of Aroclor was highest at the base of the silo. For an unknown reason, all samples collected 1 meter (about 3 ft.) from the base had low levels of Aroclor.
The levels of Aroclor 1254 in the silages from the block experiments were not as high ns those observed in silage from the silo (Figure 2). The major reason for this was that the coating containing Aroclor 1254 used on the blocks contained less Aroclor than the coating used on the silo.
All but three of the coating materials reduced the quantity of Aroclor 1254 contamination of the silage to below that of the control block. Aroclor contamina tion observed adjacent to coating I was higher than the control level. This cannot be readily explained, since this material reduced the contamination in the silo. Tho solvents in coatings III and VII probably dissolved the Aroclor in the base coat ing and caused the increased PCB residue in the silage.
The results of this block study indicate that the thickness of the cover coat ing may be an important consideration when selecting a coating to cover PCB.contami nation. This can be readily seen by comparing coating system III vs. IV and II vs. IX. In both cases, the latter coating system included both a sealer and a top coat, and the contamination was reduced. The differences in effectiveness between coatings VI and VIII, even though they are greatly different in composition, may well be the thickness of the coating. . Only a thin barrier was provided by a single coating of VI, whereas a single coat of VIII was quite thick.
These studies have not provided enough information to recommend a particular coating or type of coating to cover the PCB contamination in silos. These trials
-30-
HONS C7121Z
J
S '
3 3
I*-
. 3
f.*
8_ r
X|1
iI 8l
I 4--fs
i*T
v
k
i
8 Z 8 Si l *"
"s 1.
c non aioca
CM fOM iiaci
(MrKM llOCK
CM rMMMOCK
Fig. 1.--Parts per million (p.p.m.) of Arodor Fig. 2.--Parts per million (p.p.m.) of Aroclor
rvj 1254 (dry matter basis) in corn silage from experi 1254 (dry matter basis) in corn silage from 55-gallon
mentally coated, v;ire-brushed, and untreated sections barrels containing concrete silo blocks. The blocks
of PCB-contaninated silo. See Table 1 for a descrip were treated with a coating containing Aroclor 1254
tion of the coating materials.
and then recoated with the experimental coatings. See
Table 1 for a description of the coating materials.
M * meter
0.30 M = 1 ft
CM centimeter 2.54 CM 1 in
arc continuing to determine how long the coating will remain bonded to the silo wall ami also to determine if the Aroclor will migrate through a coating when used con tinually.
The studies have provided information about some of the necessary properties of a coaling if i-t is to be used as an effective barrier to PCB residues. These studies have indicated that it is not desirable to use a coating which contains a solvent, in which Aroclor 1254 is very soluble. It also appears that the coating thickness influences the effectiveness of the covering. .