Document meke6GLk8Vdv51pxGmveLGqk

r it Ii >i September 22, 1971 NEW FORMULA TEX-970 AC^,..TmWVNT FPEMULft READY. _MIX mLgRJTSX970 (FILLER "X") MBCRIPTION OF FBODUSTt a spmH. . jlawMatortal Aabestoa 7RF09 Vanlcide 312 Polyvinyl Alcohol Methoaol 228 Mica Aabestoa (SO-210) Land Plaster Specifications! WORKIKC PROPERTIESt Specificetions COLORt Spoolfloations' Filler for Read/ Mix Joint expound TEX-971 and TEX-972, . ' Function R.H, Spec. jgasafia& tbs/Batch Bulking agent Fungicide , Adhesive Water retention aid Anel-eracking agent Bulking agent Filler 193 4.23 8S.0 f.S ' , 162 0,35 7,0 , 7 170 ,60 12.0 /# Z * 11 m 13 ' .75 7,00 1,73 13.0 /. * ; 140.0 35.0 , tA.o 3.3 ! m -tella 170H.0 f7O,0 ; *- 100.00 2000.0 - Refer to Plant Tooting Procedure No. 32. \ Ji&fl&ma- AWPffg, ' * 62 -SR j60 Refer to Plant Tasting Procedure No, 33. Filler shall be very heavily bodied and possess fair plasticity. It shell be free of any coarse, gritty or undispersed particles. White Dried compound shall natch* color of standard sample. MOTEi A vet mix of'the filler ahall be prepared according to Formula No, TEX-971 at least twice a day or with every 6th or 7th batch of filler aanu- faotured. Thia prepared mix shall be tested and shall mast ell the specifications required of Ready Mix Joint Compound Formula Mo. TBX-971* * 4 EDOtdek 3 3tf*2 ; tJt .ft- . ` 3/, 73 4 S '??' " xo~/4-~ * Lehnert. 10.3.01-1 u DEFENDANT'S EXHIBIT I 4> SGP 0017274 January 17, 1972 Supersedes TBX-970 Dabed 9/22/71 I i I* MAPY MIX :KBMM.tK-.W ttlUJOL "X") EBSCR1PTI0N OP PRODUCT* - Pillar Ifor Ready Mix Joint Compound TEX-971 and TEX-972, FORMULA Asbestos 7RF09 Dowlotl 100 Polyvinyl Alsohol Methocel 228 ' Mica Asbestos,(SC-210) Land Plaster SpeciflootIonat Function &LJR2&* Percent Lbs/Batch Bulking agent Fungicide.. * r A. Adhesive * cf 4c*' no . Water retention aid Anti-cracking agent Bulking agent Filler 193 193 170 11 w ' m13 4*23 .15 .60 .75 7.00 1.73 85.0 4X6 3.0 12.0 13.0 tS 6* 7dT 140.0 -7o> 35.0 IIS 1110.0 f S SO : | . | j 100.00 2000.0 IO****>0 Refer bo Plane Tearing Procedure Ho, 32* flSttlgaa > J&ll&m. Average 58 toif lii, }, Specifications m0R Specifications Refer bo Plant Testing Procedure Ho* 3. Filler shall be vary heavily bodied and posseas fair plasticity. It shall be free of any coarse, gritty or undispexsed partiolea, .f ! I { White Dried compound shall mptoh color of standard sample. ! 1 WOTS* A vat mix of the filler shall be prepared according to Formula Ho, TBX-971 at least twice a day or with every 8th or 7th batch of filler manu factured. Thia prepared nix shall be teatad and- shall neat all the specifications reqauired of Reedy Mix Joint C% ompound - Formula Ho. TBX-971, ' SDOtdek ,. Lehnert 10.3,01-2 ,$*$**&/* arjr.A? jt> &&//*& <ao M+rt '4, 43/> 7 '$ 4# ?f * j?V l0t /4 SGP 0017275 t. \ i f ' * ` April 14 # 1972 Super*ados TEX-970 Dated 1/17/72 ASMS, asm raw formula Mm.HVL FILLER TEX-970 (FILLER >'X`>1 DESCRIPTION OF. PRODUCT! - filter for Reedy Mix Joint Compound TRX-971 end TEX-972, -/ FORMULA texJ&MMX Asbestos 7RF09 Dowleil 100 Polyvinyl Alcohol Methooel 228 Mice Asbestos (S0-210) Lend Fleeter ' WORKING CONSISTENCY! Specification*! working PROPERTIES Spoolfleecions COLORi Specifications _7unocion ' K.M. Spec. Percent Lbs/fritoh Bulking agent . Pungiolde * . * Adhesive <rJo* Hater retention aid Anti-cracking agent Bulking agent , rillar 9' 193 162 170.* mU . 13 4.25 . *W .60 . *75 7.00 1.75 JUl 340.00 12.00 48.00 60.00 560.00 HO. 00 WO,00 100.00 8000.00 - Refer to Plant Testing Procedure No. 32. AS 42 Jflatea.. 6a 90 toma 6JZ w Refer to Plant Testing Procedure Ho* 33* , Filler shell be very heavily bodied end possess fair plasticity, rc shell be free of any coarse, gritty or undispexsed particles. . White Dried compound shall natch aolor of standard sample UOTg{ A wet nix of the filler shell he prepared according to Formula Ho* TBX-971 at least evlea a day or with every Sth or 7th batch of filler nsnu- faotured. This properad nix shall be teeted end ehell meet ell the ' specifications required of Ready Mix Joint Compound - Formula Ho* TEX-971. J EDO}dak '7/PF1 - SG-A/o 7.n f ad&uP&h 33, / S, S4-. 3/ 7 3 49. 7F 3o, t4 *> * /<> & i n - eui Lehnert 10.3.01-3 SQP 001737$ \ < mmmA September 22, 1971 NBW FORMULA TRX-971 DESCRIPTION OF PROPUQT* - White Ready Ml* Joint Compound used for taping* covering tape* filling corner beads and spotting ' nallheads. FORMULAI Raw Haterial ** , Function ' m*M Lbs/Batch. Nslco 71-D5 Meter Preplsstioised PVA Bmulsion Filler TEX-970 Anti-foaming agent Solvent Adhesive . as me ' 185 dm 0.1 m 7.4 -91. S 1.67 om 0.00 ft 49.33 9$** **0ne batch yields it one 5 gallon pails, < 100.0 *4024vS7- ' / > ' * ` fflM6m.flaBaamogi Specifications Brabcndor Viscosity* WRKINaPROPERTIESt Specifications SpeciflostIons COLORl {Specifications Refer to Plant Testing Procedure No* 32. If paste la not of proper working consistency, * maximum of 5 ee of water per 150 grans of paste nay be added to adjust. '540 20 Refer to Plant Testing Procedure No. 33. Compound shall be plastic buttery working* and free of any coarse* gritty or undispersed particles* Materials should be free of lumps caused by Incomplete mixing. Refer to Plant Testing Procedure Mo. 35. After compound has dried* tape shall show at, least 75%. fiber tear when delaminated. . Refer to Plant Testing Procedure No* 37. There shall be no large fissure cracks In the wedge, and no cracks in the thinner half of the ` wedge. / .< White ' Dried compound shell match color of standard sample. ' EDOtdek . ., . * r Letmert 10.3,01-4 SOP 0017392 April 14, 1972 Supersedes TRY-97L Dated 9/22/71 rbaoy AOMS. TEXAS PLANT FORMULA . mm wom. DESCRIPTION OF PRODUCT; Witt a Reedy Mix Joint Compound used for taping, covering tape, filling corner beads and spotting nallhaads. ... -/ FORMULA t Raw_ Ms terlal Halco 71-D5 Water Prepiestiaiced PVA Emulsion Filler TEX-970 ,* Zmci9n Anti-foaming agent Solvent ' Adheeiva * - ` ./ **One batch yields 51 one 5 gallon pails. R.M. SgetL,, Percent H o < . 183 3.00 4*6 am 1080.00 <129 7.4 4 148.00. 1841.00 no" 100.0 3074.00 Specifications firabender Viscosity* WORH^PgOmn^t Specifications BMIHO PB0PE8TIB8I specificacions PRAg,K.RpSJ3TAHQaL COLOR! 1 Speoifioations Refer to Plant Testing Procedure No. 32 . If paste is not of proper working consistency, a maximum of 3 oo of water per 130 grams of paste may be added to'adjust. ' 040. I JO 4faltrX& Refer to Plant Testing Procedure Ho. 33. Compound shell be plastic, buttery working, and free of any coarse, gritty or undispersed ` pare Idea. Materials should be free of lumps ' caused by incomplete mixing. Refer fc<? Plant Testing Procedure Ho. 35. After compound has dried, tape shell show at least 73% fiber tear when delaminated. . Refer to Plant Testing Procedure Ho. 37. There shall be no lafge fissure erdoka in the wedge, and no1 crooks in the thinner half of the wedge. 1 * . . White Dried compound shall match color of standard sample* * . . EDOtdek -/ . Denotes change in this reissue. Lehnert 10.3.01-5 SOP 0017393 # wJ <3ntsy ae/d . / Itsej Jpoo /<.J //7. 3 a^vrx/y rd-^rtO CUaZiSf' Lehnert 10.3.01-6 / SQP 0017304 July 6, 1972 Supersedes TEX-971. Dated 4/14/72 ACME, TEXAS, PLANT POBKULA READY MIX JOINT COMPOUND tfTEX-971 (MACHINE TOOLS) DESCRIPTION OF PRODUCT - White Ready Mix Joint Compound used for taping, . .........--covocj,ttg tape, filling corner beads and spotting ttailheads. To be used in 4 gallon carton* only* FORMULA Raw Material Function R.M. Seeo. Percent Lbs/Batch Naico 71.DS Water Preplasticised PVA Emulsion Filler TEX-976 Anti-foaming agent Solvent Adhesive e . ' m 185 - ` O.L m 5.0 94*9 HL-rW- 4*4 1245.00 59 gal) U4> 100,00* I89fr0fr >7SO ** one batch yields 63 * one 4 gallon carton 100/0 mi.il WORKING CONSISTENCY Specifications Brabender Visaosity Working properties Specifications - - Refer to Plant Testing Procedure No. 32* - If paste is not of proper working consistency, a maximum of 3 cc of water per 150 grama of '* paste may be added to adjust. . --905 - 20 345 . ' - Refer to plant Testing Procedure No, 33. - Compound shall be plastic, buttery working, and , free of any coarse, gritty or undiaperaed particles* Materials should be free of lumps caused by Incom plete mixing. . BONDING ^PROPERTIES Specifications CRACK RESISTANCE Speclfieations COLOR Specifications Re Ear to Plant Testing Procedure No* 35* After compound has dried, tape shall show at least 75Z fiber tear'when delaminated. There shall be no large fissure cracks in the wedge, and no cracks in the thinner half of the wedge# , , White ' . Pried compound shall match color of standard sample/ * ' >v EDQiels 4 /a Lehnert 10.3,01-7 3GP 0017395 . August 23, 197a ` Supersedes TEX-971' >' Dated 7/6772 .. m* h ACME, TEXAS, PLANT FORMULA READY MIX JOINT COMPOUND 0TEX-971 fMACHINE*TOOLS) j,v.. Vi 'v*.' ' * DESCRIPTION OF PROPUOI - White Read/ Mix Joint Compound uaed for taping,' , ! * : \* covering cape, filling corner beads and spotting ` natlhaade, To be used In 4 gallon cartons and */ , one gallon pallSonly, ! `' FORMULA * . / Raw Material Function RtM. Spec* Peroent Lbs/Batohi * . * Nalco 71-D5 Water Preplas ticlead PVA Emulsion Filter TEH-976 4 Anti-foaming agent Solvent Adhesive * . -/ ** One batch yields ^ one 4 gallon carton - . 0.1 - ' as 996.00 <120 gals) . 185 ` m .- 5.0 92.oo * ' a /; J&2 . -1730*00 .. . - ' 100.0 2842.60 WORKlNfi CONSISTENCY - Refer to Plant Tasting Procedure No. 32* : ! Specifications - If pasta is not of proper working consistency, ' * .a maximum of 5 ea of water per 150 grams of *. ' paste may be added to adjust. , - '' r Brabender Vlaooslty - 365 - 20 '* ' . . ' WORKING PROPERTIES Specifications " bonding PROPERTIES Specifications Refer to Plant Testing Procedure No, 33* t. - \ '`A*. Compound shall be plastic, buttery working, and ! ' ' | free of any coarse', gritty or undisparaed particles.;. . .-\t Materials should be free.of.-lumps caused ;by ineom- * . ; plate mixing* . *';*/ \ * '." * Refer to Plant Testing Procedure Mo* 35* After compound baa dried, tape shall show at least 75% fiber tear when delaminated* .** '- i .. . : CRACK RESISTANCE Specif Icatiotia Specificationa EDO}els - . - . There shall be no large fissure crack*, in the wedge,- . t |' and no cracks in the thinner half of the wedge*, * 4. , - *\ ' 1; - White ' .. . .. ; - Dried compound shall match color'of tandafd aarople`/;`V , ** .... *** v '* 4li /` ' 1 " **' , ; ' *.V ` ' ' * /V' * ., /. i,, ;i. -/ denotes change # * .1* . ;V.'*> .1 -.! " V: * I. ... s |I Lehnert 10.3.01-8 t SOP 0017396 Septmebur 23, 1972 Supersedes TEX-971 Datad 8/25/72 . ACME, TEXAS, PLANT FORttUIA READY MIX JOINT COMPOUND #TaX971 (MACHINE TOQLSl DESCRIPTION OF PRODUCT - White Ready Mix Joint Compound used for taping, covering tape, filling corner bead* and spotting . - nailheuds. To be used In 4 gallon car tone, . one gallon pails, and five gallon pails. >' FOWMULA Raw Material Function R.M,' 8pec< Percent Lbs/Batch Nalco 71-D3 Motor Preplasticised PVA Emulsion Pillar TEX-976 Anti-foaming agent Solvent Adhesive 185 o.i. }0 (l^'gai*: 4.5 1.S 84.00 .(9- gala.) 95.4 *** 1758.00 ' .100,0 2842.&) ^ SO, -/ ** One batch yields A8*-t one 4 gallon carton er 45 + one five gallon pail` KORKINA CONSISTENCY Specifications Brabandor Viscosity WORKING PROPERTIES Specifications - Refer to Plant Tasting Procedure' No. 32. .. - If pasta ia not of proper working consistency, . a maximum of 5 cc of water per 150 grama of * paste may be added to adjust, - 308 - 20 * , ' 3/5 /*-/-?.* *' - Refer to Plant Testing Procedure No. 33. ; - Compound shall be plastic, buttery working, and free of any coarse, gritty or undispersed peptides; Material* should be free of lumps caused by iitcon- piece mixing. :* BON PINO PROPERTIES Specifications - Refer to Plant Testing Procedure No. 33. . - After compound has dried, tape'Shall show at least 75% fiber tear when delaminated# ' CRACK RESISTANCE Specifications There shall be no large fissure bracks in fhe podge*' and no cracks In the thinner half of. the,wedge. . COLOR Specification* - White / *. ; / ' \ . // ~ Dried compound shall natch color of standard sample.'. * , ... ' .* . ,, * , , * .. . > EDO.* els -/ denotes change .. / v , . . .. v,tfV* *, *.I ;* ,*`;t -^ .'. ` : *' *. *.*. V: -\ *.. i1 . .i* ^ r.* ', , 1:v a *-;*/.;** ............... * * ,* ` Lehnert 10.3.01-9 . y t0/Luj SGP 0017397 '/'~*9**al^*' `, March 7, 1974 Supersedes TEX-971 Dated 9/25/72 ACME, TEXAS, HAST FORMULA READY MIX JOINT COMPOUND tfTBX-971 (MACHINE TOOLS) DESCRIPTION OF PRODUCT - White Ready Mix Joint Compound uaed for taping, covering tape, filling corner beads and spotting natiheads. To be used in 4 gallon cartons, . one gallon palls, and five gallon palls. FORMULA Raw Material Function R.M. Spec, Percent Lbs/Batch < Nolco 71-D3 . Water Preplasticleed PVA Emulsion Pillar TEX-976 Anti-foaming agent Solvent Adhesive - - 163 - 0,1 4.3 95*4 4*60 996*00 (t5o gals) 84,00 1738*00 (9gals*) * 100,0 2842,60 ** One batch yields 60,1* one 4 gallon carton or 43 one flvs gallon pall* WORKING CONSISTENCY Specifications Brabender Viscosity Refer to Plant Tooting Procedure No. 32. - If peats Is not of proper working consistency, a maximum of 9 ec of water par 130 grama of paste may be added to adjust* ' - 365 - 20 . ... WORKING PROPERTIES Specifications - Refer to Plant Testing Procedure No* 33, - Compound shall be plastic, buttery working, and . free of any coarse, gritty or undiaperaed particles.* . Materials should be free of lumps caused by Incom plete mixing. BONDING PROPERTIES Specifications CRACK RESISTANCE 1 Specifications COLOR ` Specifications - Refer to Plant Tea ting Procedure No, 35. - After compound has dried, tape shall show at least 90% fiber tear whan delaminated. . Thera shall bs no large fissure cracks In the wedge, and no cracks In tha thinner half of the wedge. - White * - Dried compound shall match color of standard sample. WNGselx "/ denotes change Lehnert 10.3.01-10 SOP 0017398 i -(' '. v . * ,' ` . J May 29, 1975 Suparsadas TBX-971 Detpd t *3/7/74 1 ACME, TEXAS, PLAN? FORMULA READY MIX JOINT COMPOUND rfTRX-971 (HACHIKS TOOLS) DESCRIPTION OF PRODUCT - White Ready Mix Joint Compound used for taping, covering tape, filling corner beads and epotting nailbeada. To ba used In 4 gallon cartons, . FORMULA one gallon palls, and five gallon palls* Raw Material Function * R.M. Boae. Percent Lbs/Batch Nalcn 71-D5 Water* . Preplastlcixed FVA Emulsion .** Fillar TEX-976 Anti-foaming agent Solvent . Adhesive 125 a* 163 - 0*23 m 2.00 97.73 4.60 996.00 (120 gals) 37,00 <4 gale) 1804.40* 100.0 2842.00 ** One batch yields 40 one 4 gallon carton or 45 + one five gallon pall. WORKING C0H8I8TBN0Y ~ Specifications Srabender Viscosity - Refer to Plant Tasting Procedure No* 32* - If paste is not of proper working consistency, a maximum of 9 ao of water per 150 grams of pasta stay be added to adjust* - 365 20 WORKING PROPERTIES Specifications . . - Refer to Plant Tasting procedure No* 33. - Compound shall be plastic, buttery working, and* free of any coarse, gritty or undispersed particles. * Materials should be free of lumps caused by incoa- plate mixing* . BONDING PROPERTIES Specifications CRACK RESISTANCE Specifications COLOR Specifications - Refer to Plant Tasting Procedure No. 33. - After compound has dried, tape shall show at least 9GZ fiber tear when delaminated. there shall be no larga fissure cracks in the wedge, and no cracks in the thinner half of the wedge. - White ' . ' - Dried compound shall match color of standard sample* WNGseis ; I, / denotes change Lehnert 10.3.01-11 SOP 0017390 i> January 14, 1977 Supersedes TEX-97l Dated} 5/29/75 .. ACME, TEXAS PLANT FORMULA READY Ml JOINT COMPOUND tfTEX-971 (MACHINE TOOLS) DESCRIPTION OF PRODUCT - White Ready Mix Joint Compound used for taping, covering tape, filling comer beads and spotting ttailheads. To be.used in A gallon eartons, one gallon pails, and .five gallon pails* FORMULA Raw Material Function * RM Epee Percent Lbs/Batch Natco 71-D5 / Water ` Elvace EP-200 Ptiler TEK-976 Anti-foaming agent Solvent ' Adhesive 125 0.25 4.60 . 1129.00 (136 gals,) 185 2.00 37.00 (A gala.) a* W..73 ISOA*40 100.00 2975.00 / neOne1 batch yields 60 one 4 gallon carton or 48 one five gallon pall. WORKING CONSISTENCY Specifications Refer to Plant Testing Procedure No. 32* If paste la not of proper working consistency, a maximum of S co of water per 150 grams of paste may be added to adjust. Brabender Viscosity 365 4- 20 WORKIKO PROPERTIES Specifications ' Refer to Plant Testing Procedure No. 33. Compound shall be plastic, buttery working and free . of any coarse, gritty or undispersed partides. Materials should be free of lumps caused by incomplete mixing BONDING PROPERTIES Sped float ions Refer to Plant Testing Procedure No. 35. After compound has dried, tape aball show at least 90% fiber tear when delaminated. CRACK RESISTANCE Speei^loat Ionia There shall be no large fissure cracks In the wedge, and no cracks in the thinner half of the wedge. COLOR , . Specifications ( White ' Dried compound shall match color of atandatd sample. WNG/gvp \ */ denotes change , Lehnert 10.3.01-12 8OP 0017400 o o ` .. ' : *1 i I ACME, TEXAS, PLANT FORMULA ` READY MIX FILLER TffiC *976 fPILLBB July 6, 1972 TBX-976 MEW FORMULA ` , DESCRIPTION OP PRODUCT - Pillar Tor Ready Mix Joint: Compound TEX*970 and .TSX-971. * FORMULA Raw Material, Function R.M. flpoo. Percent Lba/Batch Dowlcil 100 Fungicide 193 Polyvinyl Alcohol 4>-Jo Adhesive 162 Gendriv 4923 Water retention aid 11 Mica Antl-cracking agent - Asbestos (80-210) Bulking agent 13 Land Plaster Filler - .15 .60 .50 7.00 3.75 88.00 12.00 46.00 40.00 560.00, 300.00 7040.00 .: * 100.00 8000.00 WORKING CONSISTENCY Specifications - Refer to Plant Testing Prooedure Mo. 32. Maximum Minimum Averase WORKING PRQPRRTIB8 Specifications 62 ' 58 60 - Refer to Plant Testing Procedure No. 33* - Pillar shall he vary heavily bodied and possess fair plasticity. It shall be free of any coarse, gritty or undiapersed particles. COLOR Specifications - White Dried Compound ahall match color of atendard sample. HOTSt A wet mix of the fillar shall be prepared according to Formula TBX-97.1 at least twice s day or with ovary 6th or 7th batoh of filler manufactured. This prepared mix shall be tested and shall meet all the specifleationa required of Reedy Mix Joint Compound - Formula No. TEX-971. EDOrels /-** 71 7#F*t 3 tf- 4tO 7-/0 -7JI 4o.f ^C, 39 34.1r7v /l. 6.4 3/. ? *3 49. 7 P &, / /O . 0 5. 3 f /fo we t & Lehnert 103.01-13 SGP 0017902 ! July 11, 197) Supercedes TLX-976 Doted 7/6/72 ACHE, TEXAS, PLANT FORMULA READY MIX FILLER TEX -976 (FILLER "X") DESCRIPTION OF PRODUCT Filler for Reedy MIR Joint Compound TEX*970 and TEX-971. ' . FORMULA Raw Material 1 Function R.M. Spec. Percent Lbs/Batoh Dowicil 75 * Polyvinyl Alcohol Gendriv 492S `Mica .. Asbestos (SG-2.IO) Land Plaster Fungicide Adhesive Water retention aid Anti-cracking agent Hulking agent PlUer 193 162 11 . * 13 - . .20 .60 .50 7.00 3.75 87.95 16.00 46.00 40.00 560.00 300.00 7036.00 100.00 8000.00 WORKING CONSISTENCY Specifications - Refer to Plant Tasting Proaadura No. 32. Max Ioann Minimum 62 38 60 WORKING PROPERTIES Specifications Refer to Plant Testing Procedure No. 33. Filler shall be very'heavily bodied and possess fair plasticity. It shall be free of any coarse, gritty or undispereed*particles* * ., COLOR . Specifications White '' Dried Compound shall match color of standard sample. NOTE: A wet mix of the filler shall be prepared according to Formula TEX-971 at least twice a day or with every 6th or 7th batch of filler manufactured. This prepared mix shall be tested and shall meet all . the specifications required of Ready Mix Joint Compound - Formula No. TEX-971. .. . EDO:alt -/ denotes change Lehnert 10.3.01-14 SOP 0017903 February 27. 1975, Supersedes TEX-976 Dated 7/11/73 . ACME, TEXAS, PLANT FORMULA . READY MIX FILLER TEX-976 (FILLER X") DESCRIPTION OF PRODUCT - Filler for Ready Mix Joint Compound TBX-970 ' ' ~ and TEX-971. ' V FORMULA Raw Material P |l ,,-- > H VaneIda ` Dowicil 75 Celvatol 3000 Gendriv 4923, Mica - Asbestos SQ~210 Land. Plaster WORKING CONSISTENCY Specifications: 1 Function KM Spec Percent Lbs/Batoh Preservative . Preservabive Adhesive Water retention aid Antl-ora eking agent Bulking agent Filler , 126 193 162 11 . -- 13 ' * .025 2.00 *175 1A.00 .60 * 40.00 .50 40.00 7.00 560.00 3-75 300.00 jam 7036.00 100.00 6000.00 l Refer to Plant Testing procedure No. 32. Maximum ' Minimum Average 62 56 ; { . 60 . WORKING PROPERTIES. \ Specifications: Refer to Plant Testing Procedure No. 33# Filler shall be very'heavily bodied and possess fair plasticity. It shall be free of any coarse gritty or undispersed particles* COLOR - White * cfpeciflcatilons; Dried compound ehall aatoii color of standard sample* * 'l NOTE! A wet mix of the. filler shall be prepared according to Formula TBX-971 at least twice a day! or with every 6th or 7th batoh of filler manufactured. This prepared mix shall be tested and shall meet all the specifications required ' ; of Ready Mix Joint Compound - Formula No ,, TBX-971. ' -/ denotes change WNGijg Lehnert 10.3.01-15 SOP 0017004 March 31, 1975 Supersedes TBX-976 Dated 2/27/75 ACME, TEXAS, PLANT FORMULA READY MIX FILLER TBX-976 (FILLER **X") DESCRIPTION OF PRODUCT - Filler for Ready Mix Joint Compound TBX-970 ---------------------- ;------------------- and TEX-971. FORMULA . Raw Material Doviioli 75 -/ Oelvatol 6ooo Qendriv 492S ' Mica Asbestos. SG-210 Land Plaster Function RM Spec Percent Lbs/Batch Preservative 186 .025 2.00 Preservative 193 *175 14.00 Adhesive 4V 162 .60 48.00 Water retention aid 11 *50 40*00 Anti-oraoklng agent --- 7.00 560.00 Bulking agent 13 .3*75 300.00 Filler --- . 67.95 7036.00 100.00 3000.00 WORKINC CONSISTENCY Spediricatibnbj Refer to Plant Testing Procedure No. 32. Maximum Minimum Average 62 53 60 WORKING PROPERTIES Specifications: - Refer to Plant Testing Procedure No. 33* Filler shall be very heavily bodied and posse si fair plasticity* It shall be free of any ooan gritty or undispersed particles. . COLOR Specifications* - White Dried compound shall match color of standard sample# . NOTE: A vet mix of the filler shall be prepared according to Formula TEX--971 et least twice a day or with every 6th or 7th batch of filler manufactured. This1 prepared mix shall be tested and shall meet all the specifications required of Ready Mix Joint Compound - Formula No, TEX-971. -/ denotes change. WHCJjats . > . ... . * ` Lehnert 10.3.01-16 . . SGP 001790$ May 29, 197r fiuparaadoc TEX-976 Dated f 3/21/75 ACME, TEXAS, PLANT FORMULA READY MIX FILLER TEX-976 (FILLER "X*) DESCRIPTION OF PRODUCT - Filler for Ready Mix Joint Compound TEX-970 :------------------------; arid TBX-971# '' FORMULA Raw Material Vanoide , Dowioil 75 Oelvatol 6000 Gendriv 492S Mica Asbestos SQ-210 Land Plaster Function RM Spoq percent Lba/Batoh Preservative Preservative Adhesive Water retention aid Anti-cracking agent Bulking agent Filler 126 193 162 223 11 13 -- .025 *175 1.00 *50 6.85 3*75 66.30 2.00 .14*00 60.00 40.00 500.00 300.00 100.00 6000.00 WORKING CONSISTENCY Speciftea t ion's; Maximum g Frooedure No. 32. Average 62 5* 60 WORKING PROPERTIES Specifications t . - Refer to Plant Testing Procedure No. 33. Filler shall be very heavily bodied and possess fair plasticity* It shall be free of any coarse gritty or undlspersed particles. COLOR Specificationst -White Dried compound shall match color of standard sample. NOTBi A wet mix of the filler shall be prepared according to Formula TH-971 at# least) twloo a day or with oytry ftb or 7th batch of filler manufactured. This prepared mix shall be tested and shall meet all the specifications required of Ready Mix Joint Compound - Formula No. TEX-971. -/ denotes ohange . UNOtalx Lehnert 10.3.01-17 SGP 0017906 January 27. 1976 Supersedes TKX-976 Datedi 5/29/75 ACMS, TEXAS, PLANT FORMULA READY MIX FILLER TEX-976 (FILLER X") DESCRIPTION OF PRODUCT - Filler for Ready Mix Joint Compound TBX-970 ------------------------ ---------- and TEX-971* FORMULA -/ Raw Material Sorbitol (Powdered) Vaneldo Dow!oil 75 Qelvatol 6000 Gendriv 4923 Mica Asbestos SQ-210 land Plaster' Function KM Suoo Borax Stabiliser preservative Preservative Adhesive 126 193 162 Water retention aid Antl-craoking agent Bulking agent Filler 223 11 13 Percent M i.o1o75 .50' 6.25 3.75 I7j_ Lbs/Bateh 31:88 .1 1d4o*.0o0o s*o 40.00 to 500.00 |1! 300.00 Vs 7032^QJ7! 100.00 6000.00 20t WORKING CONSISTENCY specifications! Refer to Plant Testing Procedure No. 32. Maximum Minimum Average 62 56 60 WORKING PROPERTIES Specifications t Refer to Plant Testing Procedure No. 33. Filler shall be very heavily bodied and possess fair plasticity, it shall be free of any ooars gritty or undispersed partiales* COLOR Specificationsj White Dried compound shall matoh color of standard sample. NOTEi ' 1 A wet mix of the filler shall be prepared according to Formula TEX-971 at Isast twice a day or with every 6th or 7th batch of filler manufactured. This prepared mix shall be tested and shall meet all the specifications required of Ready Mix Joint Compound - Formula No. TEX-971* -/ denotes change WNGjela Lehnert 10.3.0H8 SGP 0017007 April 22,'1976 &uporMift'lpC``976 .Dated* 1/27/76 ' ____ TEXAS* PLANT READY MIX FILLER TBX-" iRMLDLliAR "X") v DESCRIPTION op PRODUCT - Filler for Ready Mix Joint Compound TBX-970 and TEX-971. FORMULA Dowioil 75 Gelvabol 6qoq -/ Caisatoaol 4L1-W Mica Asbestos 80-210 ~t Land piaster Fun ot ion RM Bpeo Borax Stabiliser Preservative preservative Adhesive tm in126 Meter retention aid Anti-anaoking agent n Bulking agent - 13 Filler m . ,' .175 1 00 .50' 6.25 aa3..7oo5 . 100*00 Lbs/gat oh 14.00 !S:88 500.00 300.00 704 Q.00 6000.00 VORKINQ CONSISTENCY specifications Refer to Plant Testing Procedure Ho. 32. Maximum Average 62 50 60 WORKINQ PROPERTIBS Specifications* * - Rafer to Plant Testing Procedure Ho. 33. . Filler shall be very heavily bodied and posatas fair plaatioity. It shall be free of any ooarsej* , gritty or undlspersed particles. DOLOR Specifica.tvIonai White Dried compound shall match color of standard sample. NOTE* . . A wet mix of the filler shall be prepared aeoording to Formula TEX-971 at least twice a day or with every 6th or 7th batch of filler manufactured. This prepared mix shall be beeted and shall meet all tbs specifications required of Ready Mix Joint Compound - Formula He. TEX-971. -/ denotes change ' WNOtftVp SOP 0017908 Xehnert 10.3.01-19 November 24, 1976 Supersedes Formula TEX-976 Datedt 4/22/76 ACNE, TEXAS PLANT FORMULA ' READY MIX FILL8R TBC-976 /FILLER >ft<0 DESCRIPTION OF PRODUCT - Filler Cor Ready Mix Joint: Compound TEX-970 & TEX-971. FORMULA Raw Material Sorbitol (Powdered) / Troysan PMA-10 SEP Celvatol 6000 Galactoaol 413-t? Mica Asbestos SG-210 / Lend Plaster Function 1KM Spec Borax Stabiliser _' Preservative Adhesive 162 Water retention aid Anti-c ranking agent 11 Bulking agent 13 Filler '- Percent Lbs/Batch .300 .100 1.000 ,500 6.250 3.750 88.100 6.00 80.00 40.00 500.00 300.00 * 70*8.00 It 60 100.000 8000.00 WORKING CONSISTENCY Specifications: WORKING PROPERTIES Specifteationst COLOR Specificationst Refer to Plant Testing Procedure Mo. 32. Maximum Minimum Average 62 3a 60 Refer to Plane Testing Procedure No. 33. Filler shall be very heavily bodied end possess fair plasticity. It shall be free of any coarse, gritty or undieperaed particles* White * Dried compound shell match color of etandard sample. NtVPBt A. wet mix of the filler thill hi pPOpOtfdd SOGOfdihfi 10 Hfinull HEX*971 at least twice a day or with, every 6th or 7th batch of filler manufactured This prepared mix shall be tested and shall meet all tha specifications required of Ready Mix Joint Compound - Formula Mo. TBX-971. */ denotes change NNO/gvp Lehnert 10.3.01-20 SOP 0017910 ApviV 22y~WMr * Supersedes TBX-^76 'Dated! bf2?mr ACME, TEXASy PUNT FORMULA , READY MIX FILLER T&X-Q76 (ffTLT.BR X"V DESCRIPTION OF PRODUCT - Filler for Ready Mix Joint Compound TBX-970 * ------K------- :------------------------- and TEX-971. FORMULA Raw Material l Sorbitol ^ Powdered) Vanoido-' * Dotricll 75T^Ato p* \o Gelvatol 6000 t Galaofcosol 4i3-V Mica Asbestos SC-210 / Land Plaster Function RM Spec Percent Lbs/Batoh Borax Stabilizer ftreae**v*&4ve Preservative Adhesive Water retention aid Anti-cracking agent Bulking agent Filler 1 -m M 1 ha-- .`0 .w MfiQO* &>? 162 1.00 do.00 * .50 . AO.00 1113 6.25 -3i75. $50000..0000 --P,C,(088 ,58 100.00 dooo.oo WORKING CONSISTENCY ^pacifications* Refer to Plant Testing Procedure No. 32. Maximum Minimum Average WORKING PROPERTIES Specifications: * 62 - 56 60 - Refer to Plant Testing Procedure No. 33. Filler shall be very heavily bodied and possess fair plasticity. It shall be free of any coarse gritty or undispersed particles. COLOR specifications 1 - White Dried compound shall match color of standard sample. NOTE: A wet mix of tl\e filler shall be prepared according to Formula TEX-971 at least twice a day or with every 6th or 7th batch of filler manufactured.. This prepared mix shall be tested and shall meet all the specifications required of Ready Mix Joint Compound - Formula No. TEX-971. -/ denotes ohange WNQ:gvp Lehnert 10.3.01-21 SOP 0017909 December 1'4, 1976* Supersedes Formula TRX-976 Datedi lt/24/76 . . ACME, TEXAS PLANT FORMULA READY MIX FILLER TEX-976 (FILLER WO, * ** * DESCRIPTION OF PRODUCT - Filler for Ready Mix Joint Gompound T8K-970& TEX*971. FORMULA Raw Material mt Sorbitol (?owtfwd) Troya an PMA-10 SEP ' Galvatol $000 Oalnctoaol 413-W Mica Asbestos 80-210 -/ Land Piaster Function IRM floac Borax Stabilizer Preservative Adhesive Water retention aid Anti-cracking agent Bulking egent Filler * - 162 11 13 - Percent Lbs/Batch ,100 .106 1.000 .500 6,250 3,750 -suam 8.00 8.00 80.00 1 40,00 500,00 300,00 7064.00 100,000 8000,00 WORKING CONSISTENCY Specifications* WORKING 'PROPERTIES Specifications* COLOR Specifieatlonst Refer to Plant Tasting Procedure No, 32, Maximum Minimum ` Average $2 58 60 Refer to Plant Testing Procedure No, 33, Filler shall be very heavily bodied and possess fair plasticity. It shall be free of any coarse, gritty or undisparsed particles. White ' Dried compound shall match color of standard sample. NOTEt A wet mix of tha filler shell be prepared according to Formula TEX-971 at least twice a day or with every 6th or 7th batch of filler manufactured This prepared mix shell he tested end shall meet all the specifications required of Ready Mix Joint Compound - Formula NO, TEX-971, -/ denotes change WNO/gvp Lehnert 103.01-22 sOP 0017911 'August 25,1972, , Supersedes TEX-970 Bated 7/6/72 acme, tbxas, plant formula READY1 MIX JOINT COMPOUND WO, TEX-970 /HAND TOOLS) DESCRIPTION OF PRODUCT * White Ready Mix Joint Compound used for taping, ' ' covering tape, filling corner beads and spotting ; . v* nallheads. To be used In 4 gallon cartons only. . . . . FORMULA Raw Material Function Nalco 71-M Water ParpUfkioiaed PVA Emulsion Pillar TBX-976 * Anti-foaming agent Solvent Adhesive m -/ **One batch yeiIda 60 * ono 4 gallon carton Spec. , Peroant a . 0.1 - -. 135 5.0 - -bi Lbs/Sate|i * t * . i\, 4.60 * 929.60 (112 ghl) . # tt 92 00 , 1750.00 . . f- 100,0 2776,20 * ' - . WORKING CONSISTENCY . - Refer to Plant Tasting Procedure No. 32. !. ` Specifications - if paste is not of proper working consistency, a ' * v ` maximum of 5 cc of water per 150 grams of paste may* 4 be .added to adjust.. . i . . . ,\ -/ Svabender Viscosity - igao* + 20 . V '' ` ' " ;* * 4?*~ ' ' ` * . WORKING PROPERTIES * - Refer to Plant Testing Procedure No. 33. * .. *;* # * .. Specifications - Gompound shell be plestio, buttery working,, end ;* free of any coarse, gritty or tradlspersed part idea., Materials should be free of lumps caused by incoot- plate mixing. BONDING PROPBRTISS Specifications Refer'to Plant Tasting Procedure No, 33* .` After compound has dried, tape shall show at' . > least 75% fiber tear when delaminated, ' CRACK RESTSTANDS - Refer to Plant Tasting Procedure No, 37, There shall bo no large fissure cracks in the wedge,* and ao cracks in the thinner half of the.wedge. . COLOR Specifications - White ,,` - Dried compound shall match color of standard' sample. ,. EDO:els -/ denotes change . { ' Lehncrt 10,3.01-23 SGP 0017278 SapComber 25, id?2 Supersedes TEX-970 Dated 8/25/72 ACME, TEXASPLANT FORMULA READY MIX JOINT COMPOUND HQ. TfflC-970 (HAHP TOOLS) 7 DESCRIPTION OF PRODUCT - White Beady Mix Joint Compound used for taping, . i* * . 5'- covering tape, filling corner beads and spotting nailheede. To be used in 4 gallon cartons and five' gallon pail a. V FORMULA Function R.M. Spaa, Percent Lbs/Batch Row Material Nalco 71-D5 (later PorplastLoired PVA EmuIdion Filler TEX-976 Anti-foaming agent Solvent Adhesive as? /at MH4 gal)*. 135 4.5 & 84.00, (9 gatsi) - ..925hS*lt JLt> 117155A3.,A0A0 * 100.0 2776;20 -/ **One batch yelids 60 * one 4 gallon carton os 45 + one 5-gallon pail, - WORKING OOHSI8TgWOV Spec1ica tiona Brabendsr Viscosity WORKING PROPERTIES Specifications - Refer to Plant Testing Proodjure Ho. 32. - If paste is not of proper working consistency,, a , maximum of 5 ce of water per 150 grams of pasta may be added to adjust. . ._ -*33&+ 20 47eT * - Refer to Plant Testing Procedure Mo. 33. _ . .' - Compound shall be plastic, buttery working, and . free of any coarse, gritty or undtapereed particles. Materials should be free of lumps caused by incom plete' mixing. ' , B0HDIM0 PROPERTIES Specifications Refer to Plant Testing Precedure'Mo. 35#* After compound has dried, tape shall show at loaat 75% fiber tear when delaminated. * '* i*/*.1 \ \* * *.<*;r*,V*r1t CRACK RESISTANCE Refer to Plant Testing ProcaduraNo, 37. There shall be no large fissure cracks in the wedge, and no cracks in the thlanar half of the .wedge. . COLOR Specifications i White . Dried aompound shall match color of standard ' sample. EDO tels . -/ denotes change * . I. * * * Lehnert 1 SGP 0017279 ii Superaeclo s VfiX-970 Datad 9/23/72 ACM3, TBXAfl, PLANT FORMULA RSADY MIX JOINT COMPOUND KO* TEX-970 (HAND TOOLS') DESCRIPTION OF PROIWOT - White `Ready M1k Joint Compound used for taping, covering tape, filling corner beads and spotting nailheads. To be need In 4 gallon eartona and five gallon pails* FOHMtfLft - Function 8oep. Percent Lbs/Bapch ' Raw Material ' Nalco 71-D3 Water perplastloleod PVA Emulsion Tiller TBX-976 * Anti-foeming agent Solvent Adhesive - SI M 165 . - 0.1 4.3 ,-2M" 4.60 uu 929.60 (ifPgal) 64.00 (9 gala*) 1738*00 100,0 2770*20 **0ne batch yeilds 60 ^ one 4 gallon carton or 43 + one 3-gallon pall, WORKING CONSISTENCY Specification* Brabender Viscosity - Safer'to Plant Testing Procedure Ho. 32. - 12 paata la not of proper working consistency* a maximum of 3 eo of water per ISO grama of pea to may be added to adjust* ' - 320 + 20 WORKING PROPERTIES Specifications - Refer to Plant To a ting procedure No* 33. . - Compound shall be plastic* buttery working* end free of any coarse* gritty or undlaperaed particles. Materials should be free of lumps caused by ineomplate mining* OT>M,yTWPiBffW Specifications CRACK RESISTAMPS * COLOR Specifications WNOtelt - Refer to Plant Testing Procedure No* 35* - After eotnpound has dried* tape shall show at least 901 fiber tear when delaminated* - Refer to Plant Zesting Procedure No, 37, There shall be no large fissure cracks in the wedge* and no cracks In the thinner half of the wedge. White - Pried compound shall match color of standard sample, . / denotes change Lehnert 10.3*01-25 SOP 0017280 January 14, 1977 Supersedes TOO 970 Datedi 5/29/75 ..................... ACME,. TEXAS PLANT P0RM8LA READY MIX JOINT COMPOUND HQ. TBC-970 (BAND TOOLS) DESCRIPTION OF PRODUCT - White Ready Mix Joint compound used for taping, covering tape, filling comer beads and apottlng nallheada. To be need in 4 gallon cartons and five gallon palls* . FORMULA, Raw Haeerie1 Function' RM Rnea Percent tbs/Batch Nalco 71-DJ / Water Cloaca BP-200 PilLer TEX-976 Anti-foaming agent Solvent Adhesive 125 0.25 4.60 - - 1068.00 (128 gala.) 185 2,00 37,00 <4gala.) -ihU 180A..M 100*00 2914.00 / **0ne batch yielda 58 one 4 gallon carton or 47 oca 5 gallon pall* WORKING CONSISTENCY Spedfloatlone - Refer to Plant Testing Procedure Ho. 32. If paste is not of proper working cocaLatency, a maximum of 5 oa of water par 150 grams of paste may be added to adjust* Brabander Viscosity 520 +20 WORKING PROPERTIES Specifications Refer to Plent Tatting Procedure Ho. 33. Compound shall ba plastic, buttery working and free of any coarse, gritty or undltpateed particles. Materials should be free of lumps caused by incomplete mixing* BONDING PROPERTIES Specifications Refer to Plant Tasting Procedure Ho. 35. After compound has dried, tape aha11 shew at laaat 90% flbar tear when delaminated. CRAOK RESISTANCE Refer to Plant Testing Procedure Ho. 37. Thera shell ba no large fissure eraoks in the wedge, and no craeke in the thinnar half of the wedge* COLOR Specifications White 1 Pried compound shall match color of standard sample* WNG/gvp / denotes change i Lehnert 10.3.01-26 SOP 0017281 i September 22, 1971 NEW FORMULA TKX-972 ACMg. TBXA8 PLANT FORMULA waoir mix joinx comtobmp BO. TBX-972 (WOBIOT tool?) DESCRIPTION OF PRODUCTi '. White Ready Mix Joint Compound used for taping, covering tape, filling comer beads and epottlng nailheads. -Raw-Material Nalco 71-D5 Water Preplaatlolead PVA Emulsion Filler TBX-970 EumPAfin Anti-foaming agent Solvent " Adhesive , *' ' - 0.1 1.67 - 370.00(44 gal) 165 . 7.4 49.33 - 93.3 *iMrrtT6S,'Z, 100.00 .1034*6*- **Qne batch yields 1$ + one 5 gallon palls WORKING CONSISTBNCYt Specifications Brabender Viscosity Refer to Plant Testing Procedure No. 32. If paste la not of proper working consistency, a maximum of 5 oo of water per ISO grama of paste may be added to adjust. 385 20 . WORKING PROPERTIES Specifications Refer to Plant Testing Procedure No. 33 Compound shall be plastic, buttery working, and free of any coarse, gritty or undispersed parti cles, Materials should be free of lumps caused, by Incomplete mixing. ' BONDING EROPBRTIS81 Specifications Refer to Plant Testing Procedure No. 35. After compound bee dried, tepe shell show at least 73% fiber tear when delaminated. ORAQK .RESISTANCE! Speolfioafclons . COLORi Spool fleet ions Thera shall ba no large fissure cracks in the wedge, end no oraoke in. the thinner half of the . wedge. . * - White ` . Dried compound shall match color of standard ` . sample. EDOtdek Lehnert 103.01-27 SGP 0017509 April 14, 1972 Supersedes TEX-972 Dated 9/22/71 ACME. TEXA8 PLANT FORMULA READY MIX JOINT COMPOUND HO. TEX-972 (MACnTNB TOOtS) DESCRIPTION OF producti - White Ready Mix Joint Compound used for taping, covering tape, filling oorser beads and spotting . nailheeds. , / formula Raw HaterinI Naloo 71-DS Water Preplasticieed FVA Emulsion Filler TEX470 Function Antl-foaming agent Solvent * Adhesive - Pareant IiSs/Batali m 0*1 3.00 . 4*4 m " 1110 %00 18S 7.4 148*00 /J7.aw m 92.3 mi.oq noo 100*00 3104.00 !' / **One batch yields 31 + one 5 gallon pails WORKIKQ CONSISTENCYI Speciflostions Brabender Viscosity WORKING PROPERTIES Specifications BONDING PROPERTIESi Specifications Refer to Plant Testing Procedure No* 32* 1C paste la not of proper working oonaisteney, a maximum of 3 co of water par ISO grams of paste may be added to adjust* aofrH-eq 39* t /S Refer to Plant Testing Procedure No. 31 Compound shall be plastic, buttery working, and free of any coarse, gritty or undlapersed parti cles. Materials should be free of lumps caused by incomplete mixing* Refer to Plant Testing Procedure No* 35* After compound has dried, tape shall show at least 73% fiber tear when delaminated* CRACK RBSlflTANCEt Specifloations 4 There shall be no latge fissure oraoka in the wedge, and no oraoka in the thinner half of the wedge* ' , COLOR: Spool floations - White Dried compound shall match odor of standard sample* . I 1 ; , i EDOtdek Lehnert 10J.01-28 sap 0017510 A. ji i March 8, 1974 NEW FORMULA TEX 972 ACME, TEXAS, PLANT FORMULA READY MIX JOINT COMPOUND NO* TEX-972 DESCRIPTION OF PRODUCT - White Reedy Mi* Joint Compound4used for taping,cover ing tape, filling corner beads and spotting millboads. To be used in 4-gallon cartons and 3-gallon palls. * To ha supplied to Houston only* FORMULA Nolco 71-DS Water Preplastiaized PVA Emulsion Piller TBX-974 Function Antifoaming agent Solvent RM Spec a mt - m-- Percent Lba/Batch .23 4.60 m 929.60 <112 gsl) Adhesive -- ' ' 185 -- 3.0 94*75 92*3 <10.23 gal) 1749.00 100.00 2773.30 One batch yields 60 + one 4-gallon asrton or 43 one 3galton pail WORKING CONSISTENCY Specifications - Refer to Plant Testing Procedure No* 32. ' - If paste is not of proper working consistency, a maximum of 5 cc of water per 150 grams of paste may be added to adjust* Brabendar Viscosity - 550 + 20 WORKING PROPERTIES Specifications - Refer to Plant Testing Procedure No, 33* - Compound shall be plastic, buttery working, and free of any ooerse, gritty or undtaparsed particles* Materials should be-free of lumps caused by incom plete mixing* BOND1MO PROPERTIES Specifications - Refer to Plant Testing Procedure No* 33* - After compound has dried, tape shall show at leaat 90% fiber tear when delaminated. CRACK RESISTANCE ' - Refer to Plant Testing Procedure No* 37. There shall be no large fissure cracks in the wedge, and no cracks in the thinner half of the wedge. COLOR Specifications - White - Dried compound shall matah color of standard sample* WNG:el* Lehnert 10.3.01-29 3GP 0017811 A March B, 1974 NEW FORMULA TEX-974 \ ACME, TEXAS, PLANT FORMULA READY MIX FILLER TEX-974 DESCRIPTION OF PRODUCT - Filler for Ready Mix Joint Compound TEX-972, FORMULA Asbestos 8G210 Cendrlv 4923 Dowlcil 75 Gelvatol 6000 Asbestos Mica p80-H . * " Land Plaster TEX-25 T.P. Blend Talc Function RM Spec Fiber Filler ' Thickener Fungicide Adhesive Fiber Filler Anticraoking agent Filler - Slip Agent 13 223 193 126 9 11 m*9 m Percent Lbs/Batch 1.0 5 .2 *5 5.0 4.Q 73.8 15.0 80;o 40.0 16.0 40.0 400.0 320.0 5904.0 1200.0 100.0 6000:0 WORKING CONSISTENCY Specificationsi - Refer to Plant Testing Procedure No. 32 Maximum Minimum Averafte 62 * 58 60 WORKINQ PROPERTIES Specifications - Refer to Plant Tasting Procedure No. 33. - Filler shall be very heavily bodied and possess fair plasticity. It shall be free of any coarse gritty or undispersed particles. COLOR Specifications - White ` - Dried compound shall match color of standard sample. NOTB[ A wet mix of the filler shall be prepared according to Formula TEX-972 at least twice a day or with every sixth or seventh batch of filler manufactured. This prepared mix shall be tested and shall meet all the specifications required of Ready Mix Joint Compound Formula No, TEX-972. UNQiels i Lehnert 10.3.01-30 * SOP 0017698 A February 27. 1975 Supersedes Formula.TEX-974 Dated 3/3/74 ' . '` . t .. ACHE, TEXAS, PUNT FORMULA READY MIX FILLER TEX-974. . * DESCRIPTION OF PRODUOT ~ Filler for Ready Mix Joint Compound TEX-973. / FORMULA Raw Material , Function ' ` RM Spec Percent iWBatofr Vancide ' Asbestos 80210 ~**~--**"i* * Oendriv 4923 Dowioll 75 . Gelvatol 6000 Asbestos * Mica ]p5o-H . Land Plaster TEX-25 T.P. Blond Talc WORKING CONSISTENCY specifications* Preservative 126 j Fiber Filler -- -- ---13-- Thickener 223 Preservative 193 Adhesive * 126 . Fiber Filler 9 Anti-oraoklng agent ii! Filler Slip agent , . mum* f * *025 .a. 1.0 ' *5 .175 ' .5 5*0 4.0 73.8 15.0 j 100.0 a2o..o0_- 40.0 H.O 40.0 400.0. 320*0 5904.0 1200.0 6000,0 Refer to Paint Tooting Procedure No* 32. Maximum Minimum A"-v--o--r-aga 62 56 60 WORKING PROPERTIES Bpeoiiicafcions j ' - Refer to Plant Testing Procedure No* 33* Filler shall be very Heavily bodied and possess fair plasticity. It.shall be free of any . coarsef gritty or undispefsed (articles. COLOR ~ Specif1cafcions s - White !J Dried compound shall match color of standard sample. ' ' NOTE* * ; A wet mix of the filler shall be prepared according to Formula TEX-972 at least twice a day or with every sixth or seventh batoh of filler manufactured. .* This prepared mix shall be tested and shall meet all the specifications required of Ready Mix Joint Compound* - Formula No. TEX-972 -/ denotes change WNGljg -i i r j Lehnert 10.3.01-31 i SOP 0017699 A O Marsh 31, 1372 Acma Ho, TEC-973 HEW . . AOMB. TRyA^PUHT FORMULA . RBAOY Htx. glTXBft TO1C973 ttttMR "XY FORMULA - Pillar for Ready Mix Jains Compound TEX-974 and TEJC-973. I jtav, flay off.E.aJ, Function _ R.M. Soao. Peteant tba/Bacch Asbestos 7RF09 Dow Is 11 100 ; Polyvinyl Alcohol . * Mothocel 228 * . Mica ' Aaboatos <86-210) ' , Land Pissear Bulk!rig agent Fungloida ; Adheeive^4fw<4A^>2o- SO Water retention aid AnCl-oraeking agent Bulking agent Filler ' 193 193 162 11 13 - 4.25 .15 .60 50 7.00 1.75 UJW 212.30 **S.4>0 7.30 /J.eo 30.00 ; 25.00 So**. 350.OO 100.00! -87.30 * ?oo' 42B7 .80 f^75,00j W0RKTO6 COH3mBKCEl Specification*f 100.00 SOOOVOO tG> - Refer to Plane Zeeting Procedure Ho. 32. Kaxlrtum Minimum Amfgfl it Y WORKtHQ PROPERTIESi Specifications - -' Refer to Plane Zesting Procedure Ho. 33. > Fitter shall be very heavily bodied and possess fair plasticity. Xe shall be free of any coarse, gritty or undispersad particle.* * it /: *\ j COLOR i Specifications - White' Dried compound ahall mptch color of aeandard sample. ` .* HOTSi ' ' A wot nix of the flllor shall be prepared according to Formula Ho. TEX-974 at least twice a day or with every 6th or 7th batch of filler manufeatured. * This prepared mix shall be tested and shell meet all the epee iflent loos required of Ready Klx Joint Compound - Formula Ho. TEX-974. . , . ss.rx ju, jt^ . BDOieln ' 4k-c*vT f* 'll u Lehnert 10.3.01-32 .. . t Jdmu* * 8GP 0017595 J 1* 4 S'***cut April 14, 1972 Supersedes TEX-973 Dated 3/31/72 ACME. TEXAS PLANT FORMULA , )' RBAPQlXXJ7,XtitBR TEX-.973 (FILLER"*") JlE3GRimON^Qg_RRQDUCTl - Filler for Ready Mix .Joint Compound TEX-974 and TEX-975. formula Raw Material Function 1 R.M. Spaa. Paraont Lbs/Botch Asbestos 7RF09 Dowieil 100 '. < Polyvinyl Aloohol .' MeChocel 228 * Mica Aabeatos (30-210) * . Land Plaster '* Bulking agent Fungicide Adhesive Water retention aid Antl-praeking agent Bulking agent Filler 193 193 162 11 N 13 ' 4.25 .15 ' 60 .50 7.00 1.73 340.00 12.00 48.00 40.00 560.00 140.00 MORKIMO COHSISTBHCyi , Specifications! ; - # 100.00 . 8000.00 Refer to Blent Testing Procedure No. 32. MfiKlfflttia -HUrlCT. iemm, ' . 62 58 60 v WORKING PROFSRTXBBl ' - - Refer to Blent Testing Procedure No. 33. Specifications Filler ahell be very heavily bodied and possess fair plasticity. It shall be free off any ooerse, gritty or ondispersad particles. ' ' t COLOR! Specifications '* . - White Dried compound shall mptch color off standard sample. .* 'y' . ,m NOTEi * '* A vat nix off the filler shall be prepared according to Formula No. TEX-971 at least twice a day or with every 6th or 7th batch off filler menu** factored. This prepared mix shall be tested and ahall meet all the specific. ations required o* ff Ready Mixt Joint #Compound - Form ula No*. THX-971. C" x" ;EDOtel** , : ' ; \ 4. ' ` * . . ' / ' . `` ... . Lehncrt 10.3.01-33 80P 0017896 May 17, 1972 Supersedes Formula TBX-973 Dutad 4/14/72 v ACME. TEXAS PLANT FOIWUtA BEADY MIX FILLER TEX-973 ttIM.MU'X'!! nRRfiRT PYTOW flF PRODUCTi - Pillar for E.ady Mix Joint Ocmpound TEX-974 . and lp>"97Si fORMULA Raw Material Function^ Asbestos 7RF09 Dowtoil 100 Polyvinyl Alcohol Oandriv 4022 ' Mica Asboatos <30-210) tend Piaster Bulking agent / -^Fungicide ji.fa Adhesive - Water retention elo ' Anti-cracking agent . . Bulking agent Filler 193 193 162 w -- 1am3 Percent Lbs/flatoh 4.23 15 #60 #50 7.00 1.7$ 100.00 340.00 12,00 43.00 40,00 560.00 140.00 6860.00* 3000,00 WORKING CONSISTENGY t * Specificationst . - Refer to Maximum Plant Tasting Procedure Minimum No# 32# a Ayerse . 62 S3 60 ffOftKING PROPERTIES* Specifications COLORt Specifications Refer eo Plant Testing Procedure No. 33. Filler shall be vary heavily bodied and possess fair plasticity. It shall be free of any coarse, gritty or undispereed particles. i' White Dried compound shall mptch color of standard sample# NOTg* * A wee mix of eba filler shall be prepared according to Formula No. TEX-971 at least twice a day or with every 6th or 7th batch of filler manu factured# This prepared mix shall be tasted and shall meat all the specifications required of Ready Mix Joint Compound Formula No# TEX-971. ** ' . . ..i I ' . * .1 . : WNG:dek / *t *.'* * *. * " ` Lehnert 103.01-34 SOP 0017597 A March 31, m2 Aetna No. TKSC 974 NEW ACME. TEXAS PLANT FORMULA REAPy HIX JQlNT COMPOUND NO. TEX^7A ^HANO-YQQtSl DESCRIPTION OF PRODUCT! a* White Ready Mix Joint Compound used for taping, ., covaring tape, filling corner beade and spotting * ; nailheada. To he used in 4 gallon cartons only. formulas. Raw Macorlal ' a* * Function . Naleo 71-05 Anti-foaming agent Water ' .* Solvent , . PreplasticIzed PVA . ` Emulsion Filler TEX-VP<J " Adhesive ** e i R.K. Soee._ '- . * 133 -' i Percent 0.1 5.0 .94^9 100.0 .' Lbs/BaMh 68? . * 1162.00 ttff**, 10^00 Ufa} 1898.00 1 "# / 3161.67 : **One batch yields 65 * one 4 gallon cartons . t , i . ' WORKING CONSISTENCYt \ - Refer to Plant Testing Procedure No. 32. Specificatione If peace is not of proper working consistency, * . maximum of 5 oc oE water per 150 gratae of paste may * be added to adjust. .. Brabendar Viscosity I . -S4',.t"20 . , s/O ' i* j ? \ '] ; WORKING PROPERTIESi - Refer to Plant Testing Procedure No. 33. Specifications . * . Compound shell be plastic, buttery working, ,. and free of any coarse, gritty or undispersed .. ,particles. Materiala should be free of lumps . -. oaused by incomplete mixing. .' .. # *. . * BONDINO PROPERTIESt ' ` * - Specifleations . ' . ; ' . ,. J -Refer to Plant Testing Procedure No. 35. After compound has dried, tape shall show at least 75% fiber tear when delaminated. * . CRACK RESISTANCEi * .* ' .Refer to Plant Testing Procedure No. 37. '. There shell be no lafge fissure cracks in the ," wedge, and no oracks in the thinner half of the ' * .' *. wedge. % ' * * *\ . ** .* coLQRi ` White *' Specifications - * t . Dried.compound shall match color of standard ' * *, : : sample. . * SDQUSA8 * * * ' ** *, '* ' ' ' * . ' 4 *t *1 . " '' / , .; , . * * , . . * , i j . '' * **.. " * ' Lehflcrt 10.3.01-35 SGP 0017694 M*y 17, 1972 Supersedes Formula TEX-974 Hated 3/31/72 ACHE. TEXAS PMNT FORMULA READY fflX_JOINTJ?mg.QUKP_NO. TEX-97A.(HANp_T00L81 DESCRIPTION OF PRODUCT! . ' - Will to Raady Mix Joint Compound used for taping, oovaring capo, filling cornor beads and spotting nailheads* To ba used in 4 gallon oartona only* Row Material. Nalco 71-D5 Water 1 Proplasticized PVA Emulsion * Filler TEX-973 ' Function . Anti-foaming agent * Solvent , Adhesive m **One batch yields 65 * one 4 gallon cartons &i.tJSsaa4. Iflggonfe T*bs/BooK .. m 0.1 1162.00 fl40-g** 185 ' 5.0 mm _2i? 10.0..00 1898.00 pis**' " 100.0 J 3161.67 WORKING CONSISTENCY* Specifications Brabender Viscosity) WQRKINO PROPBRTIBS t . . Specifications BONDING PROPERTIES) . Specifications ' CRACK RESISTANCE?, SSSML Specifications t WNajdek .` -/ Denoted change Refer to Plant Testing Procedure No* 32* If paste la not of proper working consistency, a maximum of 5 c of water per 150 grams of pasta may bo added to adjust. * S40 * J/o A5 . Refer to Plant Testing Procedure No* 33* Compound shall be plastlo, buttery working, . ` and free of any coarse, gritty or undlepersed particles. Materials should be free of lumps . caused by incomplete mixing. ' Refer to Plant Testing Prooadura No* 35* After oompound has dried, tape shall'show at least 75% fiber tear when delaminated. . .Refer to Plant Testing Procedure No/* 37. There shall ba no laiga fissure oraoks in the wedge* and no cracks in the thinner half of the wedge* % .- . ' White ** Dried compound shall match oolor of standard sample* .. ` * Lehnert 10J.01-36 SOP 0017695 March 7, 1974 Met? Formula TEX 973 ACME, TEXAS, PLANT FORMULA READY MIX FILLER TEX - 973 DESCRIPTION OF PRODUCT - Filler for Ready Mix Topping Compound TEX-977. FORMULA Raw Materia} Alfresco# SG21Q Cendriv 4928 Dowioil 79 Asbaatos,7R79 . Mica p80-H Land Plaster TEX-25 T P* Blend Talc Functjtoq ,Mer HlUt RM 8see 13 Thickener 223 Fungicide 193 Fiber Filler 9 Anti-cracking agent 11 Filler SUp Agent - Percent 1,00 .50 .20 5.00 4.00 74.30 15.00 100.00 Lba/Batch 60,0 40.0 16.0 400.0 320.0 5944.0 12004 aooo.0 WORKING CONSISTENCY Specifications t tt, - Refer to Plant Testing Procedure No. 32 Maximum Minimum .* Avaraoe 62 58 60 ' WORKING PROPERTIES ' Specifications - Refer to Plant Tenting Procedure No. 33 ' - Fillor shall be very heavily bodied end potseas fair plasticity.. It shall be free of any coarse gritty or undispevaed particles. COLOR # Specifications - White - Dried compound shall match color of standard sample. KOTB: A vat mix of the filler shall be prepared according to Formula TSX-977 at least twice a day or with every sixth or seventh batch of filler manufactured. This prepared mix shell be tested and shall meet all the specifications required of Roedy Hix Joint Compound - Formula Ho`TEX-977. WNGtvlm i , Lehnert 10.3.01-37 SOP 0017999 September 11, 197$ Supersedes Formula TEX-975 Dated 5/27/75 ACME, TEXAS, PLANT FORMULA READY MIX FILLER TEX - 973 . DESCRIPTION OF PRODUCT - Fillet for Ready Mix Topping Compound TEX-977* . -/formula Raw Material Function RM Spec Vancide Preservative Qendriv 4923 Thickener ' Dowicil 75 Preservative V Asbestos Sg-210 . Mica p60-H * . Fiber Filler * Anti-oraeking agent Land Plaster TEX-25* /Filler T. P. Blend Talc / Slip agent ./ /' 126 223 19} 13' 11 2 Percent .025 .50 .175 1.25 7.50 76.55 10.00 100.00 Lbs/Batch 2.0 40.0 14.0 260.0 600.0 6264.0-y 600. 6000.0 WORKING CONSISTENCY / - Refer to Plant Testing Procedure No* $2. spe alficaone : / Maximum Minimum Average / 62 56 60 WORKING PROPERTIES Speoirioatlonsj / / - Refer to Plant Testing Procedure No* 33 Filler shall be very heavily bodied and possess fair plaetioity. It shall Be free of any coarse gritty or undispersed particles,- COLOR ' Specificationsi - white . Dried compound shall match color of standard sample,* . NOTE t "...... T A wet mix of the filler shall be prepared according to Formula TEX-977 at least twice a day or with every sixth or seventh batch of filler manufactured; This prepared mix shall be * tested and shall meet all the specifications required of ,, Ready Mix Joint Compound - Formula TEX-977 * * -/ denotes change WNG; gvp Lehnert 10.3.01-38 SOP 0017602 J April 22, 1976 ' Supersedes Formula TEX-973 Dated 9/11/73 ACME, TEXAS, PUNT FORMULA READY MIX FILLER TEX - 973 DESCRIPTION OF PRODUCT - Filler for Ready Mix Topping Compound TEX-977. FORMULA Raw Material Vancide -/ Gdlaotadol 413-W Dowioil 75 Asbestos 8<3-210 . Mica p80-H Land Piaster TEX-25 T, P. Blend Talc Function ] Preservative Thickener Preservative Fiber Filler Anti-cracking agent Filler Slip agent Spec 126 193 13 11 --. 4 2 Percent Lbe/Bafech ,025 2,0 .50 40.0 .175 14.0 }: 260.0 600.0 6264.0 -ip.oo . 800.0 100,00 6000,0 WORKING CONSISTENCY .. 6pe c ii'ica felons i Refer to Plant Testing Procedure No, 32, Maximum Minimum Average 62 5* 6o WORKING PROPERTIES Specifications* - Refer to Plant Testing Procedure No, 33 Filler shall be very Heavily bodied and possess, fair plasticity. It shall be free of any coarse > gritty or undlspersed particles. COLOR Specificationst - White Dried oompound shall match color of standard sample. NOTEi A wet mix of the filler shall be prepared according to Formula, TEX-977 at least twice a dav or with every sixth or seventh batch of filler manufactured. This prepared mix shall, be * . tested and shall meet all the specifications required of ' Ready Mix Joint Compound - Formula TEX-977* t -/ denotes change WNGt avP Lehnert 10.3.01-39 SOP 0017603 A November 24, 1976 Supersedes Formula TEX-973 Datedt 4/22/76 ACME, TEXAS PLANT FORMULA READY MIX FILLER TCX-973 DESCRIPTION OF PRODUCT - Filler for Ready Mix Topping Compound TEX-977. i FORMULA Raw Material Function RM Spec Percent Lbs/Batch Galaatosol 413-W / Troysan PMA-10 SEP Asbestos SG-210 Mica pfiO-U / Land Plaster T.P. Blend Tale Thickener Preservative . Fiber Filler Anti-cracking agent Filler Slip agent 13 11 m*. 2 .50 .10 3.25 7.50 78.65 Jt00 40.0 8.0 260.0 600.0 6292.0 800.0 100.00 8000.0 WORKING COITOIBNOT Specificationst Refer to plant Testing Procedure No, 32, Maximum Minimum 62 SS Anew 60 WORKING PROPERTIES Specificationss - Refer to Plant Testing Procedure No. 33. Filler shall be very heavily bodied and posaeas- fair plastiolty. It shall he free of any coarse, gritty or undisparsed particles. COLOR Specificationst - White Dried compound shall natch color of standard sample. NOTE: A wet mix of the filler shall be prepared according to Formula TEX-977 at least twice a day or with every sixth or seventh batch of filler manufactured. This prepared mix shall be tasted end shall meat all the specifications required of Ready Mix Joint Compound - Formula TEX-977. VNG/gvp / denotes change Lehnert 10J.01-40 SGP 001T60S Mo. is , Ayrtirtt; 1976 Supersedes Formula TEX-973 Dated Vtl/Tg- V/zytfr ACME, TEXAS, PUNT FORMULA READY MIX FILLER TEX - 973 ' DESCRIPTION OF PRODUCT - Filler for Ready Mix Topping Compound TEX-977, FORMULA Raw Material Function Iteneidc. ' Preservative 'f Galaecosol 413-Vf r Thickener Bewicidr-ygTft f * r ^preservative Asbestos do-210 Mica. jgQ-H Fiber Filler Anti-cracking agent Land plaster TEft-25 Filler T, P, Blend Talo Slip agent . . Spec Percent Lbs/Batoh 1C6 -- s25* ,50 *95* .0 dtWH 11 StO 40.0 iw:f: loSlo -- 7Uty&v&r 4264tO*7*: 2 10,00-- 600,0 100,00 6000,0 WORKING CONSISTENCY Specifications* Refer to Plant Testing Procedure Ho. 32, Maximum Minimum Average 62 56 60 WORKING PROPERTIES specifications: Refer to Plant Testing Procedure No, 33 Filler shall be very heavily bodied and possess fair plasticity. It shall be free of any coarse gritty or undispersed particles. COLOR ^"Specifications t White . Dried compound shall match color of standard sample. HOTBi A vet mix or the filler shall be prepared according to Formula TEX-977 at least twice a.dav or with every sixth or seventh batch of filler manufactured. This prepared mix' shall be ' tested and shall meet all the specifications required of Ready Mix Joint Compound - Formula TEX-977, . -/ denotes change WNQ* gvp Lehnert 10.3.01-41 SOP 0017604 A j.I /% April 12, 1973 Forriuta TEX-974 NEW ACM2* TEXAS, PLANT FORMJLA READY MIX JOINT COMPOUND TEX-974 (MACHINE TOOLS> DESCRIPTION OF PRODUCT - White Ready Mix Joint Compound used for taping, ' " coverins tape, filling cornor bead* and spotting nailheads, To bo used In 4-gallon cartons* 1-gallon pails, and 5-gallon pails* To be supplied to Houston only* . FORMULA Raw Material Function RM Sp^c Percent Lbs/Batch Nalco 71-D5 Water * Pillar TEX-976 Antifoaming agent Solvent . 0*1 m 99.9 2*0 1039*0 (125 gal) 1800.0 e 100*0 2841.0 **One batch yields 60 j* one 4-gallon carton or 45 4; one 5-gallon pall* WORKING CONSISTENCY Specifications - Refer to Plant Testing Procedure No. 32 - If paste la not of proper working consistency, a maximum of 5 cc of water per 150 grams of paste may be added to adjust. Brabender Viscosity * 365 + 20 WORKING PROPERTIES Sped fleet ions - Refer co Plant Testing Procedure No. 33 - Compound shall be plastic* buttery working, and free of any coarse, gritty or undlspersed particles* Materials should be free of lumps caused by incomplete mixing* ` BONDING PROPERTIES Specifications - Refer to Plant Testing Procedure No* 35* - After compound has dried, tape shall show at least 75% fiber tear when delaminated* CRACK RESISTANCE ' Specifications 1 * COLOR Specifications WNOiels - Thera shall be no large fissure cracks in the wedge, and no cracks in the thinner half of the wedge. - White * - Dried compound shall match color of standard sample* ' Lehnert 10.3.01-42 SOP 0017696 March 31, 1972* . Acme No.'TEX-975 NSW . ACME. TEXAS PtANT FORMULA READY MIX JOINT COMPOUND NO. TBX-975 {MACHINE TOOLS) DESCRIPTION OF PRODUCT! Whita Ready Mix Joint Compound used for taping, . " '' . 1 ..... covering tape, filling corner bead a and spotting nailheads, To bo used in 4 gallon cartons only* , FORMULA ^au Material. Nalco 71-D5 Mater . Prcplastloised BVA Emulaion Filter TEX4?C*4>7.3 fluuqi.aa Anti-foaming agent Solvent Adhesive Pare ant Lbs/Batch. S*00 id* o.t - .1245.00 4Xto-t* fS& / 185 5.0 100.00' fig* IWJHL / ? SO 100.00 , 3244 9 **Ono batch yields 55 4 o MQRKINQ CONSISTENCY! Spcflifioations Brabender Viscosity galloti cartons. Refer to Plant Testing Procedure No, 32. If paste is not of proper working coiwiaconoy, a maximum of 5 cc of water per 150 grams of paste may be added to adjust. as* jjfgP*- WORKING PROPERTIES. Specifioations Refer to Plant Tenting Procedure No. 33, Compound shall be plastic, buttery working, and free of any coarse, gritty or undispersed parti* else. Materials should be free of lumps* oaused by incomplete mixing. bonding PROPERTIES 1 . Specifications - Refer to Plant Testing Procedure No. 35. After compound has dried, cape shall show at least'75% fiber tear when delaminated. CRAOK .RESISTANCE! Specifications There shall be no lirge fissure oraoks in the wedge, and no cracks in tha thinner half of the .wedge. ' ,. ' COLOR: t . Speciflostions White Dried compound shall match color of standard sample. . ` EDOtelz* Lehnert 10.3.**43 i ; ' SOP 0017804 May 17, 1972 . Supersedes Formula TEX-975 Datad 3/31/72 ACME. TEXAS PLANT FORMULA READY MIX JOINT COMPOUND NO. TBX-975 (MACHINE TOOLS) PgSCttimOM OF PRODUCT: - WhiCo Raady Mix Joins Compound used for taping, . covering cape, filling comer beads and spotting nallheads. to be usad In A gallon cartons only. FORMULA Saw Matfitflcl, Nalco 71-D3 * Water Preplanticlead PVA Emulsion Filler TBX* 973 ,?.ync.t.tea Ant 1-foaming agent Solvent Adhesive .- &a&2aas. #e . m ' 185 . ' as faroonn Lb a/Botch 4ff. 0.1 - ' 1243.00 ft30-g /30 $.0 100.00 * f* . zSJLS. 1898.00. / 7AC --- 1 ' **0ne batch yields 63 - oda A gallon cartons. 100.00 3244.67' Wf* . WORKING CONSISTENCY: Spacifications " Brabender Viscosity WORKING PROPERTIES Specifications - Refer to Plant testing Procedure Mo. 32. . if paste la not of proper working consistency, a maximum of 5 co of water per ISO grams of ' paste may be added to adjust. - - -yflS1 T'JRT* , 376 t$ Refer to Plant testing Procedure Mo. 33. Compound shall be plastic, buttery working, and free of any coarse, gritty or undispersed parti- clea. Materials should be free of lumps caused by incomplete mixing. ROMPING PROPERTIESi Specifications Refer to Plant Testing Procedure Mo. 33. After compound has dried, tape ahall show at . least*7S& fiber tear when, delaminated. ORfrCKJSmSTANCEi Specifications A Thera shall be no large fissure creoles in the wedge, and no cracks in the thinner half of the wodgo. 44 COLOR: . Specifications White t Dried oompound shall match color of standard i sample. WMGtdek ^ /0^f .-/ Denotes ohange Lehnert 10.3.01-44 SQP 0017803 August 22, 1973 formula TBX-975 New ACME, TEXAS, PUNT FORMULA READY MIX FILLER TEX-973 DESCRIPTION 07 PRODUCT - Filler Cor Ready Mix Joint Compound TEX~978 ------- 1 " and TEX-979. FORMULA Raw Material Asbestos80210 Cendriv 4928 Dowicil 100 Celvatol'6000 Attegel 40 Mica p80-H * Land Plaster TEX-25 Function . RM Spec 'Fiber Filler Thickener 13 223 Fungicide 126 Adhesive 126 Fiber Filler Anti-cracking agent 9 11 Filler Percent 1.50 .50 .15 1.60 2.50 9.00 84.75 Lbs/Bal 120.0 40.0 12.0 128.0 200.0 720.0 6780,0 100.00 8000.0 WORKING CONSISTENCY Specifications; Refer to Plant Testing Procedure No. 32 Maximum ^ * Minimum Average * 62 58 60 WORKING PROPERTIES Specifications ' - Refer to Plant Testing Procedure No. 33 - Filler shall be very heavily bodied and possess fair plasticity. It shall be free of any coarse gritty or undispersed particles, COLOR Specifloseions - White - Dried compound shell match color of standard sample. NOTEi ' A wet mix of the filler shell be prepared according to Formula TEX "979 at least twice a day or with every aimth or seventh ( batch of filler manufactured. This prepared mix shall be tested and shall meet all the speclfioetlons required of Ready Mix Joint Compound - Formula No. TEX-979. WNOsela I : [ Lehnert 10.3.01-45 SGP 0017806 . A / . September 5, 1973 Supersedes! Pormula TEX-975 Dated 8/22/73 ACME, TEXAS, PUNT FORMULA READY MIX FILLER TBX-975 DESCRIPTION OF PRODUCT - Filler for Ready Mix Joint Compound TBX-978 and TEX-979. FORMULA Raw Material Asbuatoa 80210 GenUrlv 4928 Dowtell 73 CelVatol 6000 Ateagei 40 Mica p80-H Land Plaster TEX-23 Function RM Spec Fiber Filler Thickener 13 223 Fungicide 126 .Adhesive . 126 Fiber Filler 9 Anti-cracking agent 11 Filler Percent 1.50 .50 .20 1.60 2.30 9.00 84.70 Lbs/Batch 120.0 J3.o 40.0 f.o lfi.0 128.0 700.0 J20.0 tt 077A.O 100.00 8000.0 *oC> WORKING CONSISTENCY Specifications! Refer to Plant Testing procedure No. 32 Maximum Minimum Average 62 58 60 WORKING PROPERTIES 'Specifications - Refer to Plant Testing Procedure No. 33 ' - Filler shall be very heavily bodied and possess fair plasticity. Xt shall be free of any coarse gritty or undispersed particles. COLOR Specifications - White - Dried compound shall match color of standard sample. ` NOTE! A wet mix of the filler shall be prepared according to Formula TEX-979 at laast twice a day or with every sixth or seventh batch of filler manufactured. This prepared mix shell be tested end shall meat all the spoolfloatIona required of Ready Mix Joint Compound - Formula No. TBX-979. * WKGiele -/ indicates change Lehnert 10.3.01-46 SOP 0017807 t\ , e. V* v.,, October 22, 1973 , t Supersedes Formula TEX-978 Datad 8/22/73 * ACHE, TEXAS, PLANT FORMULA READY MIX JOINT COMPOUND, NO. TSX- 978 (HAND TOOLSV DESCRIPTION OF PRODUCT - White Ready Mix Joint Compound used lor taping, covering tape, filling corner beada and spotting nallheads* To bo usad in 4-gallon cartons and 5-gallon pails* To bo supplied to Houston only* FORMULA Baw Material Nalco 71-D5 Water Filler TEX- 975 Function RM Spec Anti-foaming agent Solvent *. percent Q.l as J&l Lbs/BateK 2*o 46 gel) 1800.0 100.00 2774.0 **One batch yields 60 one 4-gallon carton or 45 + one 5-gallon pall. WORKING CONSISTENCY Specifications * Br&bender Viscosity .-Refer to Plant Testing Procedure No. 32* - If paste is not of proper working consistency, .a maximum of 5 ce of water per 150 grams of paste may be added to adjust* *iP - 4H0 + 20 WORKING PROPERTIES Specifications BONDING PROPERTIES T 8peclfieations CRACK RESISTANCE COLOR Specifications. ' UNOiele ' -/ denotes change Refer to Plant Testing Procedure Ho* 33. Compound shell be plastic, buttery working, and free of any coarse, gritty or undiaperoed par ticles* Materials should be free of lumps . caused by incomplete mixing. .. Refer to Plant Testing Procedure Ho* 35 After compound has dried, tape shall show at least 731 fiber tear when delaminated. Refer to Plant Tasting Procedure No* 37 There shall be no large fissure eraoks in the wedge, and no cracks. in the thlnper half of the wedge* - . White , Dried compound shall match color of standard sample* Lehnert 103.01-47 SOP 0018159 October 22, 1973 Supersedes formula T&X-979 Dated 8/22/73 ACMES, TEXAS, PLANT FORMULA READY MIX JOINT COMPOUND TEX-.979 (MACHINRTOOLS) DESCRIPTION OF PRODUCT - White Ready Mix Joint Compound used for taping! * covering tape, filling cornor boads and spotting nailheade. To be used In 4-gallon cartons, 1-galIon pails, and 5-gallon palls. To be > supplied to Houston only. FORMULA Raw Material NalOo 71-05 Water Filler TBX- 975 Function Antifowning agent Solvent RM Spec Percent Lbs/Batch fS. 0.1 - 99.9 2.0 fjo 1039.0-6*06 gal 1800.0 100.0 2841*0 **0ne batch yields 60 + one 4-gallon carton or 45 one 5-gallon pall. WORKING CONSISTENCY Sped fleet lone ( - Refer to Plant Testing Procedure Mo. 32 - ill paste la not of proper working consistency, a maximum of 5 ec of water per 150 grams of paste may be added to adjust. Brabender Viscosity' - 365 + 20 WORKING PROPERTIES Specifications t . - Refer to Plant Testing Procedure No. 33 ' - Compound shall be plastic, buttery working, and free of any coarse, gritty or undlspersad particles. Materials should be free of lumps paused by lnoompletb mixing. BONDING PROPERTIES Specifications - Refer to Plant Testing Procedure No. 35* , - After compound has dried, tape ahalt show at least 75% fiber tear when delaminated. CRACK RESISTANCE Specifications .f COLOR * SpoolfleetIons ' WHOjels *.. "-/ denotes change - There shall be no. large fissure cracks in che wedge, and no creeks' in the thinner half of the wedge. , - White . Dried compound shall natch color of standard SSMOlO. . . Lehnert 10.3.01-48 * SGP 0018263 July 6, 1972 TEX-978 NEW FORMULA ACNE, .TEXAS, PLANT FORMULA READY MIX FILLER TEX*978 (FILLER "X") DESCRIPTION OF PRODUCT - Pillar Tor Ready Mix Joint Compound TEX-977 and TEX-979, FORMULA Raw Material Function R.M, Spec Percent Lbs/Batch Dowicil 100 ' Polyvinyl Alcohol Methooel 228 Mica Asbestos (80*210) Land Plaster Fungicide A-Jo Adhesivq^#'y^ Water retention eld Anti-cracking agent Bulking agent Filler 193 162 170 11 9m '. 13 ' ,13 12,00 .60 ' 48.00 .75 60,00 7,00 560.00 3.75 300.00 87.73 * 7020.00 100,00 8000.00 WORKING CONSISTENCY Specifications - Refer to Plant Testing Procedure No, 32, - Maximum Minimum Averafts 62 58 60 WORKING PROPERTIES Specifications . - Refer to Plane Tenting Procedure No, 33, - Filler shall be very heavily bodied and posses fair plasticity* It shall be free of any coaree, gritty or undlspersad particles. COLOR Specifications White Dried compound shall match color of standard sample, t NOTEi A wet mix of the flHer shall be prepared according to Formula No, TEX-979 at least twice a day or with every 6tb or 7th batch of filler manufactured. This prepared mix shall be tested and shell meet ell * the specificatlona required of Reedy Mix Joint Compound - Formula No. TEX-979, .. <Uc>r EDOtela M SG-/0 /4p* .. 3A'7 <3 ** ^>"9 Cftm f> 7 -t io< t4* - . * , . '* 40i $ l^hnert 10-3.01-49 . 7 - /O*1 7 4.' sopool8187 J~ 9 A '? *~t**s*44t. July 6, 1972 TBX-979 NEW FORMULA ACME, TEXAS PLANT FORMULA READY MIX JOINT COMPOUND NO. TEX-979 (HAND TOOLS) DESCRIPTION OF PRODUCT - White Ready Mix Joint Compound used for taping,, "1 \ '' ' ~' 1 " covering tape, filling corner beads and spotting nallhead*. ' FORMULA Raw Material Nalco 71-D5 * Water . Preplasticired PVA Emulsion Pilter TEX-978 Function R.M, Spec Anti-foaming agent Solvent IS Adhesive - ' 185 .- **One batch yields 3i ^ one 5 gallon pail Percent Lba/Bstch 0.1 -~*,00 4.d ~ 1080.00-- -(4W-al) 7.4 92.5 *niWn 7ewn -484br60 i 3?*oo J7&0 100.00 -90?4r00 * WORKING CONSISTENCY Specifications tirabender Viscosity WORKING PROPERTIES Specifications ' - Refer to Plant Testing Procedure No. 32. - If paste is not of propor working consistency, s maximum of 3 cc of water per ISO grams of paste may be added to adjust, '--540 * 20 4 70 * - Refer to Plant Testing Procedure No. 33. Compound shall be plastic, buttery working, and freo of eny coarse, gritty or undispersed particles. Materials should be free of lumps caused.by incomplete mixing, , BONDING PROPERTIES " Specifications - Refer to Plant Tasting Procedure No. 35. - After compound has dried, tape shall show at least 75% fiber tear whan delaminated. CRACK RESISTANCE Refer to Plant Testing Procedure No. 37. There shall be no largo fissure cracks in the wedge, and no cracks in "the thinner half of the wedge. . COLOR Specifications - Whito Dried Compound shall match color of standard sample. EDOjela Lehnert 103.01-50 SGP 0013260 August: 25, 1972 Supersedest T&X-979 dated 7/6/72 ACME, TEXAS PLANT FORMULA READY MIX JOINT COMPOUND NO. TBX-979 (HAND TOOLS) DESCRIPTION OF PRODUCT - Whita Ready Mix Joint Compound used for taping, covering tape, filling corner beads and spotting nailheads* ' FORMULA -/ Raw Material Function R>H Speo Percent Lbs/Batch Nslco 71-D5 Water Preplasticisod PVA Emulsion Pillar TEX-973 Anti-foaming agent Solvent Adhesive . se ** 135 y **One batch yields 45 ^ one 5 gallon pall 0.1 - * . 4.60 ^929.60 (112 gal) 7.4 92.5 100.00* 137.00 1700.00 2771.20 ' . * WORKING CONSISTENCY Specifications Brabender Viscosity WORKING PROPERTIES Specifications - Refer to Plant Testing Procedure No. 32. - If paste is not of proper working consistency, a maximum of S cc of water per ISO grans of pasta may be added to adjust. *530 + 20 4 7*" - Refer' to Plant Testing Procedure No. 33. Compound shall be plastic, buttery working, and ftoo of any coarse, gritty or undisperaed particles. Materials should be free of lumps caused by incomplete mixing. ' BONDING PROPERTIES Specifications - Refer to Plant Testing Procedure Ho. - 35. . . . - After compound has dried, tape shall show at least.,*/' 75% fiber tear when delaminated. \\ CRACK RESISTANCE Refer to Plant Testing Procedure No. 37. There shall be no large fissure cracks in the wedge, end no cracks in the thinner half of the* wedge. COLOR Specifications White Dried Compound shall match color of standard sample. EDOielz -/ denotes change Lehnert 10.3.01-51 SGP 0018261 July 6, 1972 TEX-979 NEW FORMULA ACME, TfcXAS PUHT FORMULA READY MIX JOINT COMPOUND WO. TSX-979 <HANP 10013) DESCRIPTION Qg PRODUCT - Kill be Ready Mix Joint Compound used foe taping*. covering tape* filling.corner beada end spotting ' nailheads. FORMULA Row Material Halco 71-D5 * Water Preptasticised PVA EmuIsion Filler TEX-978 Function R,M Spec Anti-foaming agent Solvent - Adhesive 185 Percent tbs/Batch 0.1 - 7.4 92,5 4,6 , 1080.00- 4U*~ggl) HjapWjl_w4A -484+tOO //* . / 37*oo t 70 O 100.00 -8094100 **One batch yields 31 ^ one 5 gallon pell woiuarn CONSISTENCY Spuolfioetloos Brabendar Viacosity WORKING PROPERTIES Spoolfleetiona - Refer to Plant Testlog Procedure No. 32, - If paste la not of proper working consistency, a maximum of See of water par 150 grams of paste moy be added to adjust. --S40 t 20 4 70 - Refer to Plant Testing Procedure No. 33. Compound shall be plastic* buttery working, and free of any coarse, gritty or uadiapereed particles. Materials should bo free of lumps caused by incomplete mixing. ' BONDING PROPERTIES Spec!floatIona - Refer to Plant Testing Procedure Ho. 35. - After compound has dried, tape shall show at least 75% fiber tear when delaminated. ' CRACK RESISTANCE Safer to Plant Tasting Procedure Ho. 37. There shall be no large fissure oracka in the wedge, and no oracks in. the thinner half of the wedge. . COLOR Specifications White Dried Compound shall match color of standard sample. EDOielx Lehnert 103.01-52 3QP001S264 fv r i August 23, 1972 ' Supersedes TBX-979 dated 7/6/72 ACME, TEXAS PLANT FORMULA READY MIX JOINT COMPOUND NO. TBX-979 (HAND TOOLS) DESCRIPTION OF PRODUCT - White Ready Mix Joint Compound used for toping, covering tope, filling corner beads and spotting naltheoda. FORMULA _j Raw Material Function R.M. Spec Percent Lbs/Batch * ' Nalco 71-D5 Water Proplastleixod PVA emulsion Filler TKX-978 Anti-foaming agent Solvent Adhesive .- w 185 ` 0.1 . 0| 7.4 92.3 .4.60 929.60 (112 gal) 137.00 1700.00 * ' . 4 -/ **One batch yields 45 ^ one 5 gallon pail 100.00 2771.20 * .. WORKING CONSISTENCY Specifications * Ufabonder Viscosity - Refer to Plant Testing Procedure No* 32. If paste is not of proper working consistency, a maximum of 5 cc of water per 150 grams of paste stay be added to adjust. ' <330 +20 WORKING PROPERTIES Specifications ^ ^ - Refer1 to Plant Tasting Procedure No. 33. Compound shall be plastic, buttery working, and froa of any coarse, gritty or undlsperaed particles. Materials should be free of lumps caused by Incomplete mixing. . BONDING PROPERTIES Specifications Refer to Plant Testing Procedure No. 33. After compound has dried, tape shall show at least'. *' 75% fiber tear when delaminated. . ' CRACK RESISTANCE - Refer to Plant Testing Procedure No. 37. There shall be no large fiesura cracks in the wedga, and no cracks in the thinner half of the wedge. . COLOR Specifications White Dried Compound shall match color of standard- sample. ' EDOjeia -/ denotes change Lehnert 10.3.01-53 . SOP 0018265 October 22, 1973 Supersedes Formula TfiX-979 Dated 8/22/73 , ACME, TEXAS, PLANT FORMULA READY MIX JOINT COMPOUND TEX-979 (MACHINS TOOLS) ` DESCRIPTION OP PRODUCT - White Ready Mix Joint Compound used for taping, covering tape, filling corner beads and spotting naillioads. To be used In ^gallon cartons, l-galIon pails, and 5-gallon palls* To be 'i supplied to Houston only* FORMULA Raw Material Function RM Spars Parcent Lbo/Batch Nalco 71-D3 Water filler TEX-975 Antifoaming agent 8olvent 0*1 - 99*9 2*0 jj0 1039.0-485 gal) 1800.0 100.0 2841.0 # **0ne batch yields 60 one 4-gallon carton or 45 + ona 5-gallon pail* WORKING CONSISTENCY Specifications - Refer to Plant Testing Procedure No* 32 - it paste is not of proper working consistency, a maximum of 5 co of water per 150 grama of paste may be added to adjust* Brabendar Viscosity - 365 + 20 WORKING PROPERTIED Specifications *1 . - Refer to Plant Testing Procedure No. 33 -Compound shall be plastic, buttery working, and free of any coarse, gritty or undlsperaad particles. Materials should bo free of lumps paused by incomplete mixing* BONDING PROPERTIES Specifications * Refer to Plane Testing Procedure No* 33* - After compound has dried, tape shall show at least 75% fiber tear when delaminated. CRACK ARBISTANCE Specifications . ` COLOR Specifications i WNGrelz - *s. t '-/ denotes change . - flic re shall be no. large fissure cracks in the wedge, and no oracka in the thinner half of the wedge. - white . - Dried compound shall match color of standard . sample. Lehnert 10.3.01-54 SGP 0018207 \ July 13, 1976 Ready Mix Pillar AK-970 NEW AKRON, NEW YORK PLANT FORMULA BEADY MIX FILLER AK-970 (FILLER "XM) PgaCRIPTION OP PRODUCT - Filler for Ready Mix Topping Compound AK-971. FORMULA Rav Material Sorbitol (Powdered) Asbestos 7RF02 Coean JTA 20 Ratcosol 2S0 HXS Mioa Asbestos (SC-210) Linestone Function Borax Stabiliser Bulking Agent Fungicide Water Retention Aid Anti-eraeking Agent Bulking Agent Filler RK Spec 9 193 170 11 18 "13 Percent .09 .90 .09 ,74 7.20 1.89 89.09 100.00 Lbs/Bs* 4.6 40.0 4.0 32.0 320.0 84.0 3960.0 4444.0 WORKING CONSISTENCY Spec1fleetions Refer to Plant Testing'Procedure No. 32. Maximum Minimum Average 62 38 60 WORKINC PROPERTIES Specifications Refer to Plant Testing Procedure No. 33. Filler shall be very heavily bodied and possess fair plasticity* Zt shall bo free of any coarse, gritty or undlspersed particles. CO^OR ' Specifications White Dried compound shall match color of standard sample. NOTE* A wet mix of the filler shall be prepared according to Formula No. AK-971 at least twice a day or with every 6th or 7th batch of filler manufactured,. This prepared mix shall be tested and shall meet, all the specifications required of Ready Mix Joint Compound - Formula No. AK-971. *?coysan PMA-10-SBP may be substituted. Uae at a loading of .18% (8 lbs/batch). HNQtgVp Lehnert 103.01-55 SGP 0017296 July 13, 1976 Ready Mix Filler AK-970 NEW AKRON, NEW YORK PLANT FORMULA REAP* MIX FILLER AK-970 (FILLER "X") DESCRIPTION OF PRODUCT - Filler for Ready Mix Tapping Compound AK-971. FORMULA Raw Material Sorblcpl (Powde red) **Asbestos 7RFQ2 *Cosan JTA 20 Natroaol 250 KXR Mica Asbestos (SC-210) Limestone Func tion . Borax Stabiliser Bulking Agent Fungicide . Water Retention Aid Anfcl-crecklng Agent Bulking Agent Filler RMSpec . 9 193 170 11 18 13 gasaa .09 .90 09 74 7.20 1.89 89.09 100.00 Lbs/Bat< 4.0 40.0 4.0 32.0 320.0 84.0 3960.0 4444.O WORKING CONSISTENCY Specifications Refer to FUnt To8tlng Procedure No* 32. Maximum Minimum . Average 62 58 60 WORKINGPROPERTIES Specifications i COLOR Specifications Refer to Plant Testing Procedure No* 33. Filter shall be very heavily bodied sod possesa fair plasticity. It shall ba free of any coarae, gritty or undisperaed particles. White Dried compound shall match- color of standard saopla. NOTE: * A wet mix of the filtev shall be prepared according to Formula No. AK-971 at least twice s day or with every 6th or 7th batch of filler manufactured. This prepared mix shall be tested and shall meet all the apealficetions required of Ready Mix Joint Compound - Formula No. AK-971. *Troysan PMA-10-SEP may be substituted. Use at a loading of .18X (6 lba/batoh). WNGi gvp Lehnert 10*3.01-56 SOP 0017300 f A January 10* 1977 Supersedes Ready Mix Filler AK-970 Dated: 7/13/76 ' Akron, new york plant formula READY MIX TILLER AK-970 (FILLER `OT DESCRIPTION OF PRODUCT - Filler for Ready Mix Topping Compound AK-971. FORMULA Raw Material -/ Sorbitol (Powdered) Asbestos 7RF02 *Coaan JTA 20 ftatroeol 230 HKR Mica Asbestos (SQ-210) -/ Limestone Function Borax Stabiliser Bulking Agent Fungicide Water Retention Aid Anti-cracking Agent Sulking Agent Filler RM Spec 9 193 170 U 18 13 Percent .07 .90 .09 .74 7.20 1.89 89.11 100.00 Lbs/Beboh 3.0 40.0 4.0 32.0 320.0 84.0 3961.0 4444.0 WORKING CONSISTENCY . Specifications Refer to Plant Testing Procedure No, 32. Maximum * Minimum Averase 62 38 60 WORKING PROPERTIES Specifications Refer to Plant Testing Procedure No, 33. Filler shall be very heavily bodied and possess fair plasticity. It shall be free of any coarse, gritty or undispersed particles. COLOR Specifications - White Dried compound shall match coLor of standard sample. NOTE: A wet mix of the filler shall be prepared according to Formula No. AK-971 at least twice a day or with every 6th or 7th batch of filler manufactured* This prepared mix shall be tested and shall meet all the speoifications required of Ready Mix Joint Compound Formula No. AK-971. *Troysan PMA-10-3EP may be substituted. Use at a loading of .18% (8 lbs/batch). wioigvp Lehnert 10.3.01-57 SOP 0017301 A r-- t July 13, 1976 Ready Mix Topping AK-971 NEW AKRON, NEW YORK PLANT FORMULA READY MIX TOPPING COMPOUND AK-971 (HAND TOOLS) DESCRIPTION OF PRODUCT - White Ready Mix Joint Compound used for topping and texturing.' . t ` FORMULA Raw Material Function * . Percent Lbs/Batch Water Nalco Elvace 1873 Filler AK-970 * . * Solvent Anti-foaming agent Adhesive Filler 0.1 4.5 95.4 100.0 2158.0 <260 gala.)* 4.0 198.0 <22.25 gala.) 4200.0 6560.0** Appcoximately 56.5 lbs/100 tba. of active ingredients (tbie may vary + 8 gatloaa per batch. **One batch yields 106 1 five gallon pail Ready Mix Jolht compound at 62 lbs/pail. WORKING CONSISTENCY Specifications for Paste - Refer to* Plant Tea ting Procedure No. 32. If paste Is not proper working consistency, a maximum of 5 cc water per 150. grams of paate may be added to adjust. Btabenden <580 20) For machine tools odd 14 gallons HgO <400 20). WORKING PROPERTIES Specifications Refer to Plant Testing Procedure No. 33. . Compound shall be pteetic, buttery working and free of any coarse, gritty or undispersed particles. Material hall be free from lumps due to' incomplete mixing. . BONDING PROPERTIES Specifications Refer to Plant Testing Procedure No. 35. After compound has dried, tape shall show at least 75% fiber tear when delaminated. CRACK RESISTANCE Specifications Refer to Plant Testing Procedure No. 37. There shall be no large fissure creaks in the wedge, and no cracks in the thinner half of the wedge. COLOR * "Specifications - White Dried compound ahall match color of standard sample. VNGigvp . r . . Lehnert 10.3.01-58 8GP 0017420 Ready Mix Topping AK-971 HEW AKRON, NEW YORK, PLANT FORMULA READY MIX TOPPING COMPOUND AK-971 (HAND TOOLS) DESCRIPTION OF PRODUCT - White Ready Mix Topping Compound used for finishing joint end spotting nail heads. FORMULA Raw Material Filler AK-970 Elvace EP 200 Halco 71D-5 Acvysol ASE-60 Water Function Filler Adhesive Defoamer Thickener Solvent RM flpao ' 163 125 147 - . Percent 93.3 6.0 .2 .3 as . Lba/Batch 4126.0 266.0 (30 gals.) 9.0 22.0 <wo *-> Approximately 96.5 lba/100 lbs. of active ingredients (this may vary 4; 6 gallons per bateh. .; **One batch yields 104 + 1 five gallon pall Ready Mix Joint compound at 62 lbs/ pail. SPECIAL MIXING INSTRUCTIONS * - Bland ingredients in following orderi l) Water 2) Elvace EP 200 3) Nalco 4) Filler AK-970 5) Mix until filler Is thoroughly dispersed 6) Add Aorysol AS8-60 7) Mix until Ready Mix is smooth - check visoosity and pH WORKING CONSISTENCY Specifications for Pasta Refer to Plant Testing Procedure No. 32. If paste la not proper working conelatency, a maximum of 5 oo water per 150 grams of paste may be added to adjust.* Brsbendori (580 20) For machine tools add 14 gallons K^O (400 + 20) pH WORKING PROPERTIES Specifications . . Minimum - 9.0 Maximum - 10.0 - Refer to Plant Testing Procedure No. 33# Compound shall be pleetio, buttery working and free of any ooaree, gritty or undlsparsed psrtielss. Matecall shall be free from lumps due to incomplete mixing. BONDING PROPERTIES Specifications Refer to Plant Tasting Procedure Mo. 35. After compound has dried, tape shall show at least 75X fiber tear when delaminated. Continued on Page 2 Lehnert 10.3.01-59 SGP 0017421 CRACK RESISTANCE Specifications COLOR Specifications Jut, W| iiii Ready Klx Topping AK-S71 NEW - Safer to Plant Tasting Procedure No. 97. Rating shall be 4 of batter* - White Dried compound shall natch color of standard sample* WHQjjr Lehnert 10.3.01-60 SGP 0017422 *4 L.7 \ t * 7 v January 16 Formula 0-970 *NEWPilV-P CHICAGO. ILLINOIS, PLANT FORMULA READY MIX FILLER 0-970 DESCRIPTION OP PRODUCT - Filler for Ready Mix joint compound C-971 FORMULA Function RM Spec Percent Lba/Batch /^Asbestos 7RF09 Dowicil 75 Celvatol 6000 Gendrlv 4923 Mica Asbestos (SQ-210)" Limestone WokKINQ CONSISTENCY specifications Bulking agent * Fungicide Adhesive Water retention aid Anti-cracking agent Bulking agent Filler 9 193 162 223 11 _ 4-Ig* lj 4.25 .20 1.00 *75 9.50 1.25 83.0$ 100.00 170.00 8.oo 40.00 30.00 380.00 50.00 3322.00 4000.00 Refer to Plant Testing Procedure No. 32. Maximum ` Minimum Average . WORKING PROPERTIES specifications ' COLOR Specifications 57 53 55 Refer to Plant Testing Procedure No. 33. Filler shall be very heavily bodied and possess fair plasticity. It shall be free of any coarse, gritty, or undispereed particles. - White Dried compound shall match color of standard sample. A~ NOTE* y,,p uvv. ti Cu>iTTur^t) , MSmS Af A MMlmJ* (\\o ABS/Lvun/J, A wet mix of the filler shall be prepared according to Formula No. 0-972 at least twice a day or with every oth or 7th batch of filler manufactured. Ihis prepared mix shall be tested and shall meet all the specifications required of Ready Mix Joint Compound - Formula No. 0-972. 1.7IT * WNGjjg Lehnert 103.01-61 SOP 0018S48 A ik** 1*?, Krr Jvamvr-36* 1975 IFIEoriMmutolaTjv0-yI71I i* fisr ` CHICAGO, ILLINOIS, PLANT FORMULA READY MIX JOINT COMPOUND 0-971 (HAND TOOLS) DESCRIPTION OF PRODUCT - White Ready Mix Joint Compound used for taping, ...."" "' " topping, and texturing, 5peoial-1w coat- 'formula For-trial* shipnente^-only. FORMULA RawMaterial Function . Percent Lbs/Batoh Water Nalco Elvaoe 1*75 Filler 0-970 Solvent Anti-foaming agent Adhesive Filler -- *2 2.0 97.8 1024*00 (128 gala.)* 4*00 39.00 (4.4 gals.) 1950.00 , 100.0 3017.00## #Approximately 56.5 lbs/100 lbs, of active ingredients (this may vary 8 gallons per batch. ##0ne batch yields 50 1 five gallon pall Ready Mix joint compound at 62 lbs/pail. WORKING CONSISTENCY ` 8p9cYiTcations for Paste - Refer to Plant Testing Procedure No. 32. If paste Is not proper working ooneietenoy, a maximum of 5 ec water per 150 grams *of paste may be added to adjust. Brabenderj (540 t 20) For maohine tools add 10 gallons HgO. (400 t 20) WORKING PROPERTIES Specifications - Refer to Plant Tasting Procedure No. 33, Compound shall be plastic, buttery working, and free of any coarse, gritty, or undispersed particles. Material shall be free from lumps due to incomplete mixing. Spec - Refer to Plant Testing Procedure No. 35* Aftercompound has dried, tape shall show at least 90$ fiber tear when delaminated. CRACK RESISTANCE ' Specifications - Refer to Plant Testing Procedure No. 37. There shall be no large fissure cracks in the wedge, and no oraoks in the thinner half of tne wedge, COLOR - White Dried compound shall match color of standard sample. WNOtjg Lehnert 10,3.01-62 SQP 0018549 . . Supersedes* Formula 0*970 ' Dated* ty*i/76 ,. CHICAGO, ILLINOIS, PLANT FORMULA READY MIX FILLER C-970 . . DESCRIPTION OF PRODUCT * Filler for Ready Mix joint compound C-976, ` . FORMULA . Raw Material * Sorbitol Asbestos SG210 *Asbestos 7RP02 ^TDowioil 73 . . Hamleo 267 Natrosol 250 HER Mien P80-F -/ Serialte Mice GP-F-2 / Linestone. Functiop Borax Stabiliser Bulkipg Agent Bulking Agent Preservative Adhesive Water Retention Aid Anti-Cracking Miae-Extender Filler SI 16 9 193 23 170 11 * 13 ` Percent; Lba/Batch .090 4.00 1.575 1.575 .360 .563 70.00 70.00 16.00 26.00 .430 20.00 6.731 6.751 300.00 > 300.00 91.8631 100.00 3939.004444,00 WORKING CONSISTENCY Specification* WORKING PROPERTIES Specifications COLOfr Specifications Refer to Plant Tee ting Procedure No. 32. Maximum Minimum Average 57 53 53 Refer to Plant Testing Procedure No. 33* Filler shall be very heavily bodied and possess fair plasticity. It shall ha free of any coarse, gritty, or undlspereed particles. White Dried compound shell match color of standard sample. NOTE* A wet mix of the filler shell be prepared according to Formula No. 0*971 at leaat twice a day or with every 6th or 7th hatch of filler manufactured. This prepared mix shall be taetad end shall neat ell the specifications required of Reedy Mix Joint Compound - Formula No. 0*971 rtjfr . yw a AT A- kOA'&t - s&f> Of % 3d St/te. &A-TQU f denotes change '. WNOrgvp . * .' ' ,' i . Lehnert 10.3.01-63 S6P 0018527 January*!0^ 1977' Supersedes: '7ormuZa C-970 I Dated: .12/1/76 CHICAGO, ILLINOIS, PLANT FORMULA READY tflr rii,t.ttR 0-970 t .. ' DESCRIPTION OP PRODUCT Pi Her for Seedy Mix Joint compound C-976.,. * # FORMULA ` . ' . Haw Material -/ Sorbitol Asbestos 8G210 *Asbe*tos 7RF02 1 -/ Troysen PMA-10-SEP . ; . Hsmlco 267 Natrosol 250 HSR Mica P80-F Sariclta Mica GP-P-2 -/ Limas tone ' . Function Borsx Stabiliser Bulking Agent Bulking Agent Preservative . Adhesive Water Retention Aid Anti-Cracking Mica-Extender Pillar . RM Soac - 18 9 Percent .067 1.575 1.575 .180 23 .585 170 .450 11 6.731 - . . .,-6.251-. !i___ _ . 82.066. 100.00 Lbs/Batch 3.00 70,00 70.00 2IM 20.00 300.00 30O,.Q0. ulttLSS. 4444.00 WORKING CONSISTENCY Specifications WORKINO PROPERTIES Specifications f COLOR Specifications - Refer to Plant Testing Procedure No. 32. Maximum Minimum Averasa 37 53 55 Refer to Plant Testing Procedure No. 33. Pillar shall be very heavily bodied and possess fair plasticity. It shall be free of any coarse, gritty, or undispersed particles. White Dried compound shall match color of standard sample. NOTB; A vat mix of the filler shall be prepared according to Formula No. C-971 at least twice a day or with every 6th or 7th batch of filler manufactured This prepared mix shall be tested and shall meet all tha specifications required of Ready Mix Joint Compound - Formula No. C-971. -/ denotes change WNQ; gvp Lehnert 10.3.01-64 SOP 001851S A- - S *YO I0i M77 Supetiecfo'aT^ 'Formula c-970 Dated; 13^3/76 U| /7b CHICAGO, XLLXN018, PLANT FORMULA BRADY MIX FILLER C-970 I DESCRIPTION Of PRODUCT - Filler for Randy Mix Joint compound C-976. - FORMULA Raw Material Sorbitol Asbestos SG210 r *AabasCos 7R702 ./ ** Dowieit:75 *. -1 tuW'*/ *S> ' . Tfamico 267 v Natroaol 250 HXR Mioa PBO-F SecLeite Mica GP-F-2 --/ Limestone Function Borax Stabiliser Bulking Agent ' Bulking Agent . Preservative Adhesive Water Retention Aid Anti-Cracking Mi ca-Extender Filler RM Spec Percent m 4 t>(* 7 /090- 18 1.575 * 9 1*575 .393. 23 .360 .585 170 .450 U /m 6.751 6.751 13& 10U. 8b: 363. 100.00 Lbs/Batohj 4r00* 70.00 70.00 46*0026.00 V.O 6 20.00 * 300.00 300.00 -asto.-to 4444.00 $(,<* 7 ,ffl^ffq,S2g,3?8jEgcy Specifications WORKING PROPERTIES Specifteatlone COLOR Specifications Refer to Plane Tea ting* Procedure Ho. 32. Maximum Minimum * Average 57 33 55 Refer to Plant Testing Procedure No. 33. Filler aba11 bo very heavily bodied end poaseas fair plasticity* It shall be free of any coaraa, gritty, or undisparaed particles. White Dried compound shall match color of standard sample* NOTE; A wet mix of the filler shall be prepared according to Formula No. C-971 at least twice a day or with every 6th or.7th batch of fillar manufactured. This prepared mix shall be tested and shall meat all the specification* required of Ready Mix Joint Compound - Formula No. 0*971* ffl?n llflij flL u lnmlitig */ denotes change WNQt JP ' Lehnert 103.01-65 . S6P 0018S3S fU- (\. rv January 10 1977 * . Superseded Formula C-976 Datedt 7/21/7.6 CHICAGO, ILLINOIS. PLANT FORMULA RgAPI MU JOINT COMPOUND 0-976 (HAND TOOLS) DESCRIPTION OF PRODUCT - White Ready Mix Joint Compound used for taping, topping, and texturing. FORMULA Haw Material /Water Naloo -/ EWio BP-200 Filler 0-970 Function a' Percent Solvent --- Anti-foaming agent .1 Adhesive 6.4 Filler 93.S Lbs/Batoh 103 8.00 (125 gals.)# 2.00 134.00 <15.0 gal*,) 1950.00 * 100.0. 3124.00## #Approximately 56,5 lbe/100 lbs, of active Ingredients (this may vary I a gallons per batch. . - `H ' .' -/ ##One batch yields soil five gallon pail Ready Mix Joint compound at 62 lbs/pail. \ WORKINC CONSISTENCY Specifications for Paste - Refer to plant Testing Procedure No. 32. If paste is not proper working consistency, a maximum of $ co water per 150 grams of paste may be added to adjust. Brabendart (5#0 + 20) For machine tools add 10 gallons Hj>0. (400 20} WORmO PROPERTIES 'Specifications - Refer to Plant Testing Prooedure No. 33* Compound 'shall be plastic, buttery working and* free of any coarse, gritty or undispersed articles. Material shall be free, from lumps ue to incomplete mixing. BOtroiKQ PROPERTIES Specifications - Refer to Plant Testing Procedure No. 35* After compound has dried, tape shall show at least 90# fiber tear when delaminated. CRACK RESISTANCE .. Specifications - Refer to Plant Testing Procedure No. 37. There shall be no large fissure oraoks in the wedge, and no cracks in the thinner half of the wedge. COLOR - White Dried compound shall, match color of standard sample. VINO i gvp -/ denotes 0hangs Lehnert 10.3.01-<5d 8QP 0018521 I .I . 711<?77 Supersedes formula C-976 Dated M2m ?/* 'ht> CHICAGO, ILLINOIS. PLANT FORMULA READY MIX JOINT COMPOUND 0-976 (HAND TOOLS) DESCRIPTION OF PRODUCT - White Ready Mix Joint Compound used for taping, * ' topping, and texturing. .' FORMULA Raw Material . * Function Percent Lba/Batch -/ Water Naloo -/ llvaca 4FW . <-* 't.oo * Filler C-970 Solvent ` Ant1-foamlng agent Adhesive Filler - /c-iP 1G&MQ (4^0 gals.)** 1 2i00 6.4 jJ<2wju5L 1d9&5'0S,LoZo <l5* 100.0, -m 6i00*t D* Y ^Approximately 56.5 lbs/100 lbs. of active Ingredients (this may vary Z & gallons per batch. 1 s* * -- / **Oge batjjh fields iftrt 1 five gallon pail Ready Mix Joint compound WORKING CONSISTENCY ^Specifications for Paste - Refer to Plant Testing Procedure No. 32. If paste Is not proper working consistency, a maximum of 5 00 water per 150 grama of paste may be added to adjust. Brabenderi (580 t 20) For machine tools add 10 gallons HgO. (400 20) WORKING PROPERTIES Specifications - Refer to Plant Testing Procedure No. 33. Compound 'shall be plastic, buttery working and free of any coarse, gritty or undlspersed particles. Material snail be free from lumps due to incomplete mixing. BONDINQ PROPERTIES Speoifications Refer to Plant Testing Procedure No. 35* After compound has dried, tape shall show at least 90$ fiber tear when delaminated. CRACK RESISTANCE Specifications - Refer to Plant Testing Procedure No. 37* There shall be no large fissure craoks in the wedge, and no cracks in the thinner half of the wedge. COLOR -White Dried compound shall match color of standard sample. . WNQi gvp -/ denotes change SOP 0018538 74AJ. f7//.fr7 7.V-H76-- Formula C-979' ****** *~/z//V- CHICAGO, ILLINOIS PLANT FORMULA RgADY MIX JOINT COMPOUND C-979 (HAND TOOLS) DESCRIPTION OF PRODUCT * Whits Ready Mix Joint Compound used for taping, topping *-( nnd texturing* (Special asbestos free formula Cor all one ' gallon ready mix and selective ,iva gallon shipment only*) FOMM Raw Material Function HM Spec Percent Lbs/Batch Filler C-978 Blvace *$75* Cfr too Halco 71D-3 Aorysol ASR-60 -- / *ttetar Filler Adhesive Dafoamer Thickener Solvent 185 125 147 92.8 6.5 .2 .5 -- 1950.0 156.0 <15.25 gale.) 4.0 10.0 //OVHGQtO <&$*gels.) 100,0 3P*0tO** tzotf ^Approximately 56.5 lbs/100 lbs. of active ingredients (this may vary + 8 gallons per batch. . ** One batch yields 51 + l five gallon pail Ready Mix joint compound at 62 tbs/pail. SPECIAL MIXING INSTRUCTIONS - Blend ingredients in following orders 1) Water 2) Elvac*tWAC^ loo 3) Nalco 4) Filler C-978 5) Mix until filler ia dispersed 6) Add Aerysol ASB-60 7) Mix until Ready Mix is smooth - pumping viscosity should be 480 + 20 to allow for 24 hour viscosity build of 100 pts. WORKING CONSISTENCY Specifications for Paste - Refer to Plant Testing Procedure No. 32. - If paste is not proper working consistency, a maximum of 5 go water per 150 grams of paste stay be added to adjust. , Brabeiufar: (580 + 20) For Machine tools add7 gnllon.s RgO (400 + 20) pH Minimum - 9.0 Maximum - 10.0 (24 hra.) WORKING PROPERTIES J "" ' - Refer to Plant Testing Procedure Ho. 33. . Compound shall be plastic, buttery working and free of any coarse, gritty or undlspersed particles, Material shall be free from lumps due to incomplete mixing. WNGsgvp Continued on Page 2. Lehnert 103.01-67 SOP 0018840 ir i , Ready Mix Topping m-$n MBW W, ITgXtW, PLANT FORMULA READY MIX TOPPING CDMPOuibA-971 (HAND TOOLS ^ DESCRIPTION QT PRODUCT - White Ready Mix Topping Compound used for finishing Joint and spotting nail heads* FORMULA Raw Material <S A Filler JR-970 Blvace BP 200 Nalco 7ID-5 Acvyaol ASE-60 Water . Function RM Spec Filler Adhesive 185 Defoamer 125 Thickener 147 Solvent ' ' mm Jg Tit/ 6.0 } 4b ease Lbs/Batch 84<i0 {Mgala*) HrrO&* gSSfefeCWO gals*) Approximately 56,5 lba/100 lbs. of aetlve ingredient* (this may vary + $ gallons par batch* One batch yield a %n five gallon pail Ready Mix joint oompound at 62 lbs/ pail. . SPECIAL MIXING INSTRUCTIONS Blend ingredients In following orderi 1) water 2) Elvaee BP 200 3) Nalco eu 4) Filler Jfifc-970 5) Mix until filler la thoroughly dispersed ' 6) Add Aerysol ASB60 7) Mix until Ready Mix is smooth - check viscosity and pH . WORKING CONSISTENCY Specifications for Paata Refer to Plant Tasting Procedure Mo. 32. If paste is not proper working consistency, a maximum of 5 cc vacer per ISO grams of paste may be added to adjust* Brabendevi <360 4* 20) For machine tools add gallons H0 (400 + 20) ' *" pH Minimum - 9*0 Maximum - 4W10 WORKING PROPERTIES Specifications -Refer to Plant Testing Procedure Ho* 33* Compound obeli be plastic, buttery working sod free of any coaraa, gritty or undisparsed partiolea* Matesail shall be free from lumps due to incomplete mixing* BOND IMP PROPERTIES Specifications , ` Refer to Plant Testing Proeadure Ho* 35* After compound has dried, tape shall show at laast 73% fiber tear when delaminated* Continued on Page 2 tehnertio.3.01-68 3OP 001680 SBACK RESISTANCE Spacifications COLOR Specifications July 19, */? R*dy HI* Topping 4K-971 * NSW Rafsr to Plant Tea ting Procedure No. 37, Rating shall be 4 of better. Whitt Dried compound shall match color of standard sample. WNOijr ____ _____ _ ii Lehnert 10.3.01-69 SOP 0018509 k* i i \ `--v t q: *f . 'I July--!Vrl976 * - ymtnrSupersedes* Formula C-973 Dated* ?/* CHICAGO, ILLINOIS, PLANT FORMULA READY MIX FILLER 0-973 DESCRIPTION 0? PRODUCT Filler for Ready Mix Topping compound C974 Rev Materiel /* Sorbitol Asbeetoe SO 210 Asbestos 7RF02 -' rfSTOotfiell 73 - Natrosol 250 HXR Mice P80-F Serialte Mica GP-F-2 Limestone * *** Function * Borax Stab!liter1 Bulking Agent Bulking Agent ' Preservative Water Retention Aid Anti-Cracking Mica-Extender Filler KK Spec 16 9 193 170 11 m 13 -' Percent --mr 1.75 1.75 .20 .73 7.30 12.00 73.93 100,00 70.00 70.00 6.00 30.00 300.00 460.00 3038.00 4000,00 WORKING CONSISTENCY Specifications WORKING PROPERTIES Specificsclone COLOR Speoifications - Refer to Plant Testing Procedure No, 32. Maximum Minimum 57 S3 53 Refer to Plant Testing Procedure No. 33. Filler shell be very heavily bodied end poetess fair plasticity, it shell be free of any coarse, gritty, or nndlftpersed particles. White Dried compound shell match color of standard sample. NOTHi A wet mix of the filler shall be prepared according to Formula No. C-974.et least twice a day or vith every 6th or 7th batch of filler manufactured. This prepared mix shall be tested end shall meet all the specifications required of Reedy Mix Joint Compound - Formula No* G-974. . ^ s T A* ~tO* ' 2^ StlUSTlTUT/J), LA*.* &r y AS54S//j*/|na.M. WNOigvp Lehnert 10,3.01-70 SOP 0018S2S A (~ January 10, 1977 Supersedes! Formula C-973 Dated! 12/1/76 > CHICAGO, ILLINOIS, PLANT FORMULA READY MUt FILLER C-973 DESCRIPTION OF PRODUCT - Filler for Ready Mix Topping compound C-974. FORMULA Ram Material Function * Sorbitol Borax Stabiliser Asbestos SO 210 / Bulking Agsat Asbestos 7.RF02 * * Bulking Agent Troyaan PMA-10-SKP Preservative Natrosol- 230 RKR - Water Retention Aid Mica P80-P Anti-Cracking Scrtcite Mice GP-P-2 Mica-Extender Limestone Filler RMBpec 18 9 as 170 U ' 13 Percent ro75 1.73 1.75 .20 .75 7.30 12.00 75.973 Lbs/Batoh m'TM 70,00 70.00 8.00 30.00 300.00 480.00 3039.00 100.00 4000.00 WORKING CONSISTENCY Specifications WORKING PROPERTIES Specifications COLOR Specifications Refer to Plant Testing Procedure No* 32. Maximum Minimum Average 37 33 33 Refer to Plant Tenting Procedure No. 33. Filler shall be very heavily bodied and posses* fair plastioity. It shall be free of any coarse, gritty, ox undispersed partiolas. White Dried compound shall match color of standard sample. NOTE: A met mix of the filler shall be prepared according to Formula No. C-974 at least twice a day or with every 6th or 7th batch of filler manufactured. This prepared mix shall ba tested and shall meat all the specifications required of Ready Mix Joint Compound - Formula No. C-974. --/ denotes change WNGtgvp Lehnert 10,3.01-71 SOP 0018519 n Bupetaerfeai formula 0-073 s Oitidt ?^/76 f rtf1 l7e> CUtOAOO, XM.IHOI8, PLANT FORMtttA RBAPV H3X PlttSa 0-973 pgfiCaiPttQK OP PRODUCT - Pillar for Batty Mix Topping coupound 0-974. Ra* Materiel V&eor * Aebestoa flo 210 Albateea_7RF92 . 'HSttaSil 230 KKR Mica f60-P Sarlolta Mica 0P-P-2 -/ Limeatoae i Function - Bora Stabiliser . Bulking Agent Bulking Agent .Preservative water Retention Aid Anti-Cracking Hloa-Rxtender Filler .T RH.Bpoo Paroant - i5Tvr IS 1.73 9 1.75 >443-- .20 170 .73 11 7.50 12.00 13 7g47ff>3^>1' 100.00 Lba/Batoh JOi't,, o 70.00 70.00 8.00 30.00 300.00 480.00 3038700 4000.00 1*0^80 C0W1WIMW Speeificetioae VmtM PROPgRTlgg Specification* Specification! Refer to Plant Tearing Procedure No. 32. Nwlmum HSuigaa 37 53 Average 35 Refer bo Plane teeting Prooedure Ho. 33. filler shell bo very heavily bodied and possess fair plasticity, it ahalt bo free of any coarse, gritty, or ncidltparted partielea, Wilts Dried compound shell match color of standard cample. ' HOVEt A Vet ate of the filler shall be prepared according to formula Ho. 0-974 at leaae tele# a day or with ovary 6th or 7th bateh ef filler menufeecured, Ttaia prepared mix shall be coated end shall vest ell the specification! required of Reedy Nix Joint Compound - formula No, 0-974. I irrl'll If-MW^ restituted;-- Udo-iklPft` n 1 n -0> -/ denotes change WNOti/ Jp 80p 0016538 Lehnert 10.3.01-72 February 6, $975 * Supersedes <3-97$ Dated 1/16/75, CHICAGO, ILLINOIS, PLANT FORMULA READY MIX FILLER C-976 (FILLER "X) DESCRIPTION OF PRODUCT- Filler for Ready .Mix joint compound 0-976 FORMULA Function . RM Spec Percent Lbs/Batch Asbestos 7RF09 Dowicil 75 Gelvatol 3000 /Oendrlv A92S Mica * : Asbestos (S0-210) Limestone Bulking Agent Fungicide Adhesive Water retention aid Anti-cracking agent Bulking agent Filler 9 193 162 223 11 13 4.25 20 .40 .75 9.50 1.25 93.6s 100.00 170.00 8.00 16.00 30.00 380.00 50.00 3346.00 4000.00 WORKING CONSISTENCY . Specifications WORKING PROPERTIES Specifications COLOR Specifications - Refer to Plant Testing Procedure No. 32. Maximum Minimum Average 57 53 55 - RefSr to Plant Testing Procedure No. 33. Filler shall be very Heavily bodied and possess fair plasticity. It shall be free of any coarse gritty or undlspersed particles. White Dried compound shall match color of standard sample* NOTEt A wet mix of the filler shall be prepared according to Formula No. C-979 at least twice a day or with every 6th or 7th batch of filler manufactured. This prepared mix shall be tested and shall meet all the specifications required of Ready Mix Joint Compound - Formula No. C-979* -/ denotes change WNGjel* Lehnert IO.3.OL73 SGP 0018547 l^'Ao TWO* Supersedes Formula 0-974 Dated t 3/23/76- 7/?.f/76 CHICAGO* ILLINOIS, PLANT FORMULA READY MIX TOPPIHO COMPOUND C-974 CHAMP TOOLS) 1 DESCRIPTION OF PRODUCT - White Ready Hlx Topping Compound used for topping and spotting railheads. ,. . a FORHOA Ram Materials / Water Nslco -/ Elvace-4SW- Filler C-973 ^ -too ,, .* RM Function * 8pac Solvent -- Anti-foaming Agent 125 Adhesive 195 Filler . Paroent Lbs/Batch ~ /^loeOoSao gala)* 0,1 2.00 -- 4.5 92.00 (10.5 gala) 93.4 1950.00 100,0 3124*00** V 20: 7 *Approxlmately 54.4 lbs/100 lbs. of motive ingredients (this may vary + 8 gallons per batch). **0ne batch yields 50 + 1 five gallon pail Ready Mia Joint compound at 62 Iba/pall. WORKING CONSISTENCY Specification for Paste: - Refer to Plant Testing Procedure No* 32. If paste is not proper working consistency, e maximum of 5 cc water per 130 grams of pasta may be added to adjust. Brabendor: 580 * 20 Per machine tools add 6 gallons R2O (400 + 20) W0RKIHQ_PROPERTIES "spa ci teat Iona: - Refer to Plant Testing Procedure No. 33. Compound shall be plastic, buttery working, and free * of any coarse, gritty, or undispersed particles Material shall be free from lumps due to incomplete mixing. ' BONDING PROPERTIES Specifications: Refer to Plant Testing Procedure No. 35. After compound has dried, tape shall show at least 751 fiber tear when delaminated. CRACK RESISTANCE Specifications: Refer to Plant Testing Procedure No. 37. There shall be no large fissure crack* in the wedge, and no cracks la the thinner half of the wedge. COLOR Specifications: - White ' Dried compound shell natch color of standard sample. WNGsgvp ./ denote* change Lchnert 10J.01-74 SOP 0018537 June 21, IV 73 Supersedes Formula V-977 Dated 1/23/73 MILFORD, VIRGINIA PLANT READY MIX JOINT COMPOUND V-977 (MACHINE TOOLS) DESCRIPTION OF PRODUCT - White ready mix joint compound used for taping, topping, and texturing FORMULA . Raw Material Function RM Spec Percent Lbs/Batoh Water PVA Emulsion NALCO Asbestos 7RF09 Dowioil 100 FV Alcohol KThlckner Mica Asbestos SO--210 Limestone Calgon T Solvent Adhesive Antifoaraing Agent Bulking Agent Bactericide Adhesive Thiokner " Anticracking Agent Bulking Agent Filler Slip Agent 185 7.40 125 .10 9 3.92 193 .14 162 .74 170or223 .9 11 6.46 id 1.62 13 78.70 229 --zSl 144,0 2.00 78.00 3,0 15,0 14*0 129.0 32.0 1575,0 4*0 100.00 3140.0 *Hatrosol 250 HXR or Gendriv 4925 Approximately 56.5 lbs/100 lbs. of active ingredients (this may vary -4 gallons per batch* **0ne batch yields 50 + 1 five gallon pail Ready Mix joint compound at 62 lbB/jttile . WORKING CONSISTENCY ~ Refer to Plant Testing Procedure No* 32. Specifications ror Pastes If paste is not proper working consistency, , a maximum of 5 00. water per 150 grama of paste . may be added to adjust* Brabendert 385 - 20 WORKING PROPERTIES Specifications Refer to Plant Testing Procedure No. 33. Compound shall be plaatlo, buttery working, and free of any coarse, gritty, or undispersed particles. Material' shall be free from lumps due to Incomplete mixing* CRACK RESISTANCE specifications CO: fipiRecifioaclone RDOtjg Refer to Plant Testing Procedure No. 35* After compound has dried, tape shall'show at least 75* fiber tear when delaminated. Refer to Plant Testing Procedure No, 37* There shall be no large fissure cracks in the wedge, and no cracks in the thinner half of the wedge White '. Dried compound shall match color of standard sample. Lehnert 10.3.01-75 S6P 0018144 July 12, 1973 Supersedes Formula V-977 Dated 6/21/73 MILFORD, VIRGINIA PLANT READY MIX JOINT COMPOUND 7-977 (MACHINE TOOLS) . * DESCRIPTION OF PRODUCT - White ready mix joint compound used for taping, topping, and texturing FORMULA Ray Material Function RM Spec Percent Lbs/Baboh Water PVA Emulsion NALCO Asbestos 7R709 Dowioil 100 PV Alcohol *Thidcnor Mica Asbestos 80-210 Limestone Calgon T Solvent Adhesive Antifoaming Agent Bulking*Agent Bactericide Adhesive Thickner Antioraoking Agent Bulking Agent Filler Slip Agent 185 7.40 125 .10 9 3.92 193 162 19 74 170orS43 .69 11 6.46 18 1.62 13 78.65 229 -ji 148.0 2.00 78.00 4.0 15.0 14.0 129.0 32.0 1574.0 4.0 100.00 3140.0 *Natrosol 250 HXR or Gendrlv 4925 {Approximately 56.5 lbs/100 lbs* of aotive ingredients (this may vary - 4 gallons per batch* . **0ne batch yields 50 + 1 five gallon pail. Ready Mix joint compound at 62 lbs/pail s * WORKING CONSISTENCY - Refer to Plant Testing Procedure No* 32. Specifications for Pastes If paste Is not proper working consistency, a maximum of 5 cc. water per 150 grams of paste . ' may be added to adjust* Brabenderj 365 - 20 WORKING PROPERTIES Specifications --Refer to Plant Testing Procedure No* 33* Compound shall be plastio, buttery working, and free of any coarse, gritty, or undispersed ^articles. Material shall be free from lumps ue to incomplete mixing* BONDING PROPERTIES Specifications - Refer to Plant Testing Procedure No* 35. After oompound has dried, tape shall show at least 75^ fiber tear when delaminated* ORAOK RESISTANCE specifications - Refer to Plant Testing Procedure No* 37* There shall be no large fissure araoks in the wedge, and no oraoka in the thinner half of the wedge. COLOR "^Specifications EDOijg - White Dried compound shall matoh color of standard sample. Lehnert 10.3.01-76 SOP 0018145 i* * i v, tv/> Suitftr'iod'u: I'Virm.iI'j 7-077 Dated 7/12/73 MILFORD, VIRGINIA, PLANT HFAPy MIX JOINT COMIOIINP y-977 ( MACHINE TOOLS) PKSCRtt'TTOM OF PRODUCT - White ready mix Joint compound u.jod P* r taping, topping, and texturing FORMULA Rat/ unto rial Water PVA EmulsionNALCO Aoboutoo 7RF09 "/ Troyean Cmp-lO-Sop PV Alcohol *Thickner Mica Asbestos S0-21U -/ Limestone Function Solvent Adhesive Antifoaming Agent Bulking Agent Bactericide Adhesive Thicknor Anticracking Agent Bulking Agent Filler W Spec prirc'-n*. .* / .'.ch IS 5 7.40 125 .lO 9 193 .1) 162 .7* I70or223 ,(>') 11 6./,'. is 1.62 13 7B.9.7 l u *<(i3^gal 1/ *A r * / / M# / i' v .; 100.00 3140.0 *Natroool 250 HXR or Qendriv 4925 . "Approximately 56,5 lbs/100 lbs. of active ingredients (this m/ vary * 4 gallons per batch). **One batch yields 50+1 five gallon pail Ready Mix joint compound at o2 lba/pail. WORKIHQ CONSISTENCY specificaclond ior Pastes Brabtmdert Refer to Plant Testing Procedure Ko. 3:. If paste is not proper working consist *,ney, * a maximum of 5 cc. water per 150 gratae of paste may be added to adjust. 3S5 20 V/ORKinO PROPERTIES 3 Specifications Refer to Plant Testing Procedure No. ' . * Compound shall be plastic, butterv w>ikutr, and free of any coarse, gritey, c* *K `p.rsed particles. Material shall be free fiv:. lumps due to incomplete mixing. BOaNOpIoMcPiilPoRaOlPioErRjTaIES Refer to Plant Testing Procedure Hu*. . After compound has dried, tape shall rl ow at least 75# fiber tear when delaminated. . CRACK RESISTANCE specifications Refer to Plant Testing Procedure No. ... There shall be no large fissure cracks in lit* Wedge, and no oracka In the thinner half cf the wedge. . . j COLOR apSolflcaMons A Whi te Srletl ooiapourol stall roa&Qti color or standard sample WHOsjg Lehnert 10.3.01-77 8Qpoo18146 k-*Vt- January 15# 1974 Superseded Formula 7-977 Dated 10/ld/73 MILFORD, VIRGINIA, PLANT "'IADI Mil JOINT COMPOUND V-977 ( MACHINS TOOLS) ZW.wnZQ* OF PRODUCT - White ready mix Joint compound used for taping, topping, and texturing 7<V?V*** A nw ?!atorial Function RM Soso Percent Lba/Batoh -/ *Abater HVA Emulsion ::aloo Amatos 73F09 Trnvsan Cmp-10-Sep ?V Alcohol ratroeol 250 HXR ::ica Actest03 30-210 Limestone Cll^on rf Solvent Adhesive Antlfoamlng Agent Bulking Agent Bactericide Adhesive Thiokner Anticracking Agent Bulking Agent Filler Dispersant 135 125 9 170 U Id 1? 229 74100 3*92 .10 A 6ft6 1.62 M- 100.00 1140(136^1* 14*.0 2.0 7d.o 2.0 15.0 14.0 129.0 J2.0 1576.0 4.0 3140.0##* ^Approximately *>6.'5 lbs/100 lbs."of aotive ingredients' (this may vary h gallons per batch) batch yields 50 + 1 five gallon pall Ready Mix Joint compound at 62 lbs/pail. . WORKING CONSISTENCY ixn oil icat ions1 for ` Paste; Refer to Plant Testing Procedure No. 32, If paste Is not proper working consistency, a maximum of 5 oo. water per 150 grams of paste may be added to adjust. -/ Srabejider; 400 i 20 WORKING PROFSRTIES 3pecif*Lentions Refer to Plant Testing procedure No. 33* Compound shall be plastic, buttery working, and free of any coarse, gritty, or undlapersed partIdea. Material shall be free from lumps due to incomplete mixing. BONDING P30PBRTIB3 Refer to Plant Testing Procedure No. 35. After compound has dried, tape shall show at least 759* fiber tear when delaminated. C3 C!C RESISTANCE !<XiC 11 i /Ions - Refer to Plant Testing Procedure No. 37. There shall be no large fissure cracks in the Wedge, and no oraoka in. the thinner half of the wedge. GOTO?. otecifications - White Dried compound shall match color of standard sample. Lehnert 10.3.01-78 SOP 0018143 . February 22, 1974 Supersedes Formula V-977 Dated 1/15/74 MILFORD. VIRGINIA. PLANT READY MIX JOINT COMPOUND V-977 (MACHINE TOOLS) DESCRIPTION OF PRODUCT - White ready mix joint compound used for taping, topping, and texturing -/ FORMULA Raw Material * Water PVA Emulsion NALCO . Asbestos 7RF09 Troysan Cmp-10-Sep PV Alcohol Natroool 250 HER Mica Asbestos S0-210 Limestone Calgon T Function RM Spec Percent Lbs/Bafcoh Solvent Adhesive Antifoaming Agent Bulking Agent Bactericide Adhesive Thiokner Anticraoking Agent Bulking Agent Filler Dispersant 185 125 9 193 162 170 11 18 13 229 7.00 .10 3.92 .10 .75 ^70 8.79 1.25 77.19 raro.2c0r lUO(136fial 140.0 2.0 78.0 2.0 15.0 14.0 175.0 25.0 1537.0 apg4l.o0uHr ** Approximately 56.5 lbs/100 lbs. of aotovs Ingredients (this may vary 4 gallons per b&toh). *#* one batch yields 50-1 five gallon pall Ready Mix joint compound at 62 lbs/pail. Jpacifications or Pastet Refer to Plant Testing Procedure No. 32. If paste Is not proper working consistency, a maximum of 5 00 water per 150 grams of paste may be added to adjust, . Brabendert 400 - 20 WORKING PROPERTIES opacifications - Refer to Plant Testing Prooedure No . 33. Compound shall be plastic, buttery working, and free of any coarse, gritty, or undispersed Sarticles. Material shall bo free from lumps ue to imcomplete mixing. BONDING PROPERTIES Bpecii'icationa - Refer to Plant Testing Procedure No. 35# After compound has dried, tape shall snow at least 75 fiber tear when delaminated. CRACK RESISTANCE specifications -Refer to Plant Testing Procedure No. 37. There shall be no large fissure cracks in the wedge, and no' cracks in the thinner half of the wedge. COLOR Specifications -- White Dried compound shall match color of standard sample . . Lehnert 10,3.01-79 sOP00'"*149 1\ - *W March 6, 1974 Supersedes Formula V-977 - Dated 2/22/74 MILFORD t VIRGINIA* PLANT J READY MIX JOINT COMPOUND V-977 (MACHINE TOOLg) DESCRIPTION OF PRODUCT - Whits ready mix joint oompound used for . taping, topping, and texturing FORMULA Raw Material **Water PVA Emulsion NALCO Asbestos 7RF09 Troysan Cmp-10-8ep PV Alcohol Natrosol 250 HXR Mica Asbestos 50-210 Limestone Calgon T Function RM Spec Peroent Lba/Bfttoh Solvent Adhesive Antifoaming Agent Bulking Agent Bactericide Adhesive Thiokner Anticracking Agent Bulking Agent Filler Dispersant 1*5 125 9 193 162 "2 IB 13 ?29 7.00 .10 3.92 .10 .75 .70 $.79 1.25 77.19 .20 100.00 U40(136gal 140.0 2.0 7B.0 2.0 15.0 14*0 175.0 25.0 153F7.0 ___ 4ai O____ yrvt[,'.'OWIN' ** Approximately 56.5 lbs/100 lbs. of aotove ingredients (this may vary 4 gallons per batch). *^w^0nObb^th^yields 50 1 five gallon pail Ready Mix Joint compound at WORKING CONSISTENCY specifications for Pastes Brabender: WORKING PROPERTIES specifications .. . BONDING PROPERTIES bpeciiicabions CRACK RESISTANCE specifications COLOR specifications lw - Refer to Plant Testing Procedure No. ,32.. if paste is not proper working consistency, a maximum of 5 co. water per 150 grams of pasts may be added to adjust. , 400 20 - Refer to Plant Testing Procedure No. 33. Compound shall be plastic, buttery working, and free of any coarse, gritty, or undlspersed particles. Material shall be free from lumps due to Incomplete mixing. Refer to Plant Testing Procedure No. 35. After compound has dried, tape shall show at least 90 fiber tear when delaminated. Refer to Plant Testing Procedure No. 37* There shall be no large fissure cracks in the wedge, and no' cracks in the thinner half of the wedge. .. White Dried compound shall match color of standard sample. ,. Lehnert 10.3.01-80 . BGP 0018150 I'iUy *U, Supersedes Formula V-977 Dated 3/6/74. MILFORD* VIRGINIA, PLANT J READY MIX JOINT COMPOUND V-977 (MACHINE TOOLd) DESCRIPTION OF PRODUCT - White ready mix joint compound used for taping, topping, and texturing -/ FORMULA Raw Material ""Water PVA Emulsion NALCO Asbestos 7RF09 Troysan Cmp-10-Sep PV Alcohol Natrosol 250 HXR Mica Asbestos 80--210 Limestone Calgon T Funotion RM Spec Percent Lba/Bato^ Solvent Adhesive ' Antifoaming Agent Bulking Agent Bactericide Adhesive Thlckner Antloraoklng Agent Bulking Agent Filler Dispersant id! 12! 170 11 IS 13 229 7.00 .10 3.92 10 1140(136gal 140.0 2.0 75.0 2.0 S.79 1*25 -77*565 . .20 175.0 25.0 1544.9 3T3S8mnr "" Approximately 56.5 lbs/100 lbs. of aotove Ingredients (this may vary 4 gallons per batch). *** One batch yields. 50-1 five gallon pail Ready Mix joint compound at 62 Ibs/pall. Specified! ons for Pastes Refer to Plant Testing Procedure No. 32. If paste la not proper working consistency, a maximum of 5 oc. water per 150 grams of paste may be added to adjust. . ' Brabendert 400 t-20 WORKING PROPERTIES specifications Refer to Plant Testing Procedure No. 33* Compound shall be pi&stio, buttery working, and free of any coarse, gritty* or undlapersed Sartiolee* Material shall be free from lumps ue to lnfcomplste mixing. , BO jpacifiestides Refer to Plant Testing Procedure No* 35* After compound has dried, tape shall ehow at least 90 fiber tear when delaminated* CRACK RESISTANCE specifications - Refer to Plant Testing Procedure No. 37* There shall be no large fissure craoke In the wedge, and no` cracks in the thinner half of the wedge. . COLOR Specifications -White .. Dried compound shall match color of standard sample. `. . WNCi jg -/ denotes change Lehnert 10,3.01-81 SGP 0018151 Jinuoty 27, 1972 MEW FORMULA AX-SOI Continued Brabander Viscosity 480 - 10, Viscosity can be adjusted by addition of water, reduction of nix water, or by addition of ASE-60 In snail amounts* It la bast to hold back a small amount of water to be added if the viscosity is coo high. ASE-60 nay be added to chicken the nix should too mueh water have been added. Should It be necessary to add ASS-60, the pH must again be checked eince ASS-60 la addle and its addition will lower pH. Remember, changes in the water content affect flow properties as well as the wet density,, WORKIKO CHARACTERISTICSi Shall extrude easily from tube and form a uniform bead that does not sag or run* OPEN TIMS Refer to Plant Testing Procedure No. 114 f `. ' NETTING CHARACTERISTICS t Refer to Plant Testing Procedure Ho. US TENSILE STRENGTH - Refer to Plant Teatlug Procedure No* 116 ATjgALTtttTg - Refer to Plant Testing Procedure No* 34, Adjust with small quantities of AMP * Specifications t Maximum Mininun, Average 9.0 7.7 DENSITY Specifications: - 10.75 lbs/gal ' 10*65 lbs/gal * Case weight should be 35 lbs* ^ 1 lb, 7*9 10.7 Ibs/gal EDO:el*' Lefanert 103.01-82 SGP 0016181 fv February U, 1972 Supersede* AK-501 Dated 1/27/72 AKRON, NEW YORK, PLANT FORMULA DRYKALL ADHESIVE AK-SOl DElCRIPTION: - Drywall scud adhesive. Provisional formula for salvaging formula AK-955. FORMULA: Raw Material Function RM Spec. Percent Lbs,/Batch Akron Stud Adhesive AK-955 . Water Solvent >- Advawet 33 Watting agent * Water Solvent Clay Filler Asbestos SO 210 Filler Resin EB-12 Adhesive Emulsion RA-315 Adhesive 217 Propasol Filming Agent Dlbutyl Phthalate Plasticiser Water Solvent Acrysol ASH-60 Thickening egent AMP 95 'pH Buffer 225 54.9 1.6 1.0 6.0 9.0 0.8 8.2 5.2 1.1 0.8 7.3 3.5 0-4 100.0 <102 cases of small tubes 2818.Oor 78k cases 82,0 (9.8 gals.) 31.0 (6.1 gals.) 308.0 (37 gals.) 462.0 41.0 421.0 (56 gals.) 267.0 (30 gals.) 56.0 (7.8 gals.) 41.0 (4.7 gals.) 415.0 (50 gals.) 180.0 (21 gals.) 31.0 (395 aala.) 5133.0 YIELD - One batch yield 480 gals. MIXING PROCEDURE - Extract AK-935 directly into mixer and proceed in the following.order: ^ 1) Add water followed by the Advawet 33, 2) Mix for five minutes, , 3) Add the water (2nd addition) followed hjf thd filSy fllld SSbOSCOSt 4) Kix for a further 30 minutes. 5) Add the following ingredients allowing each ingredient to be thoroughly blended before addition of the next Ingredient. . Resin SB-12 Emulsion RA-315 Propasol Dibutyl phthalate ' . . . . ' A) Add water and Acrysol ASE-50 (may be added simultaneously) AMP 95 . VISCOSITY - Refer to Plant Testing Procedure No. 109. Specifications': 120 to 300 Brabender unit Leftnert 10.3*0^^ SGP 0018182 ' '. . February 11, 1972 Supersede* AK-501 (Coot.) Dated 1/27/72 Brcbaacar Viscosity Viscosity con be adjusted by addition of water, reduction of mix water, or by addition of ASE-60 in small amounts* It is bast to hold back a small amount of water to be added If the viscosity is too high* ASE-60 may be added to thicken the mix should coo much water have been added* Should it be necessary to add ASS-60, the pH must again be cheeked since ASE-60 la acidic and its addition will lower pH. Remember, changes in the water content affect flow properties as well as the wet density* 1 ' WPRKIX3 CHARACTERISTICSt Shall extrude easily from tuba an<J form a uniform bead that does not sag or run. OPEN* TIK3 ' - Refer to Plant Testing Procedure Ho* 114 8EITXS3 CHARACTERISTICSi Refer to Plant Testing Procedure Vo. 115 TEKSHE STRENGTH - Refer to Plant Testing Procedure Vo. 116 ' Al&ALISITY - Refer to Plant Testing Procedure Vo* 34* Adjust with small quantities of AMP Specifications} Maximum Minimum Average 9.0 DEK3ITY Specifications: -11.20 lbs/gal 7.7 10,60 lbs/gal 8.3 10,9 Ibs/gal Casa weight should be 35 lbs. * 1 lb. * * t EDOtels Lehnert 10.3.01-84 i SGP 0016183 Fobruiry 18 1972 Supersedes AX-501 Datad 2/11/72 AKROX, X2W YORK, PIAXT FORMULA DRYWALL ADK2SIV3 AK-SOi _ mS^.IPTIOX: Dryvsll stud adhesive. Provisional formula fox salvaging formula AX-953. FOigyLA: Raw Materiel Function Akron Stud Adhesive AX-955 4* Water Advowee 33 Solvene Wetting agent '* Hater Solvent Clay Filler Asbestos 66 210 Filler - Resin 3-12 Adhesive Emulsion BA-3IS Adhesive 217 Propaaol Filming Agent Dibutyl Phchalaca Plasticizer We tar Solvent Acrysol ASE-60 Thiokanin8,agent . AK? 95 'pH Buffer 223 Percent Lbs./Batch _ 54.9 1.6 1.0 4.0 9.0 0.8 $.2 5.2 1.1 0.8 7.3 3.5 0.6 100.0 (102 cases oi 2818,0 or-78* cases 82.0 (9.8 gals.) 51,0 <6.1 gals.) 3oa.o (37 gels.) 442.0 41.0 421.0 <54 gals.) 267.0 (30 gals.) 54.0 <7.8 gals.) 41.0 (4.7 gals.) 413.0 (50 gals.) 180.0 (21 gals.) 31.0 (395 gals.) 5173.00 cubai Y1SLP - One batch yield 480 gals. ' * yiXIRg PBOCEDSRg - Extract AX-955 directly into mixer and proceed in the fallowing order: , . N ' 1) Add water followed by the Advavat 33* 2) Kix far five minutes. 3) Add the water (2nd addition) followed by the clay and asbestos. A) Xix for a further 30 minutes. 3) Add the following ingredients allowing each ingredient to be thoroughly blended before addition of the next ingredient. Rosin 3-12 Emulsion RA-315 Propscol Dibutyl phthalaee t `, . 4) Add water and Aorysol ASS-40 (say be added simultaneously) ' i'2 93 * VISCOSIT Y - Refer to': Plant Teasing Procedure go. 109. Scarifications: 120 to 3C0 Brabender unit Lehnert 10.3.01-85 i 3GP OOKM84 February 18, 1972 Supersedes AK-501 (Coot.) Da cad 2/11/72 Srcfeondor V1acoaitv Viscosity can be adjusted by addition of water, reduceIon of nix water; or by addition of ASE-60 in small amounts. It Is bast to hold back a small amount oi water to be added ll the viscosity is too high. ASZ-60 may be added to thicken the mix should too ouch water have been added* Should it be necessary to add ASS-60, the pH must again be checked since ASE-60 is acidic and its add!don will lower pH* Remember, changes in the water concent affect flow properties as well aa tha wee deneiey* - '* KOamc CHARACTERISTICSi Shall extrude easily from tube and fora a uniform bead that does not sag or run. OPES - Refer to Plant Testing Procedure Ho. 114 WETTING CHARACTERISTICS; Refer to Plant Testing Procedure Ho. 113 TSHSILS BTREKQlg - Refer to Plant Testing Procedure Ho. 116 ALKALINITY - Refer to Plant Teeting Procedure Ho. 34. Adjust with small quantities of AM?' ' Specifications: Maximum 'e 9.0 . DENSITY Specifications*. -11*20' lbs/gal ` Mtoimun - 7.7 . 10.60 - lbs/gal Average 8.3 10.9 Ibs/gal Cose weight should be 35 lbe. * 1 lb. t .. SD0:els t Lehnert 10.3.01-86 SOP 0018183 January 28, 1972 AKRON FORMULA. AK-502 NEW ARSON, NEW YORK, PLANT FORMULA DRYWALL ADHESIVE AK-302 _ DESCRIPTION * Dryvall stud adhesive FORMULA Saw Material Water Cslgon-T R thylane Olycol Advawet-33 Atomics Limestone Clay BP03 Asbestos 5G210 Resin EB-12 Emulsion SA-315 Propasol Dlbutyl Phchalate Water Aorysol ASE-60 AMP-95 Biocide 290 Function RM 8oec Percent Lbs./Batch Solvent Wetting Agent Solvent Wetting Agent Filler Filler Filler Adhesive . Adhesive Filming Agent Plasticiser Solvent Thickening Agent pH Buffer Fungicide 11 182 220 217 225 12.0 0.1 3.0 0.9 27.0 9.0 0.8 8.0 30.0 1.6 0.8 2.8 3.8 0.5 0.3 617.0 (74 gals.) 5.0 154,0 (16.6 gals.) 46.0 (5.5 gals.) 1398.5 462.0 41.0 410.0 (55 gals.) 1541.0 (173.0 gals.) 51.0 (7.0 gals.) 41.0 (4.7 gals.) 144.0 (17.3 gats.) 195.0 (22.4 gals.) 26,0 (3.3 gals.) 1.5 100.0 5133.0 YIELD - One batch yield 4B0 gals. . MIXING PROCEDURE - . '. 1) Add water (first.addition) Celgon-I , Ethylene Glycol and Advawst 33* 2) Add Atomite, Clay, Asbestos and mix for 30 minutes 3) Add the following Ingredient* allowing each Ingradlant to ho ' thoroughly blended before addition of the next Ingredient* Reein EB-12 Emulsion RA-315 Propasol Dlbutyl Phchalate - 4) Add water (second addition) and Aeryso l ASE-60 (may be added simul taneously 5) Add AMP 95 * Biocide-290 Lehnert 10,3.01-87 SOP 0016188 A January 20, 1972 ___^ AKRON FORMULA AK-JO* HEW C0NT1KUB& VISCOSITY - Refer to Plant Testing Procedure No, 109 Specifications: 460 t 10 Brabender unit Brabender Viscosity 480 t IQ. Viscosity can ba adjusted by addition of vs ter, reduction of mix water, or by addition of ASE*60 in small amounts* It Is boat to hold back a small amount of water to ba added if the viscosity la eoo high. ASE-60 may ba added to chicken the mix should too much water have been added. Should it be neeeaaery to add AS~60, Che pH must again be checked sine* ASE-60 is acidic and its addition will lower pH. Remember, changes in the water content affect flow properties as well 48 the wet density; WORKING CHARACTERISTICS i Shall extrude easily from cube and form a uniform bead thee does not sag or run. OPEN TIMS - Refer to Plane Testing Procedure Ho. 114 GETTING CHARACTERISTICS: Refer to Plant Tasting Procedure No. 115 TENSILE STRENGTH - Refer to Plant Tasting Procedure Ho. 116 ALKALINITY ' - Refer to Plant Testing Procedure Ho. 34. Adjust with small quantities of AMP Specification*: Maximum Minimum Average 8 7.7 7.9 DENSITY Specifications: 10.75 lbs./gal 10*65 lbs./gal 10.7 lbs./gal Case weight should be 35 lbs. ^ 1 lb. &DO:els , Lehnert 103.01-88 SOP 0016189 August 15, 1972 Supersedes AK-502 Dated 1/28/72 AKRON, NEW YORK, PLANT FORMULA PKYWALL ADHESIVE AK-502 DESCRIPTION - Drywall stud adhesive FORMULA Raw Material Function RM Soec. Percent Lbs./Batch < Water Calgoa-T * Ethylene Glycol Advawet-33 Atomite Limestone Clay BPC3 Asbestos SC210 Resin SB-12 ' Emulsion RA-315 Propasol Dibutyl Phthelate Water Acrysol ASE-60 AMP-95 Biocide 290 Solvent Wetting Agent Solvent Wetting Agent Filler Filler Filler Adhesive Adhesive Filming. Agent Plasticiser Solvent Thickening Agent pH Buffer . Fungicide' 11 182 220 ` .. 217 225. *4 12.0 0.1 3.0 0.9 27.0 9.0 0.8 8.0 30.0 1.0 0.8 2.8 3.8 0.5 - 0.3 617.0 (74 gals.) 5.0 154.0 (16.6 gals.) 46.0 (5.5 gals.) 1398.3 462.0 41.0 . 410.0 (55 gals.) 1541.0 (173.0 gals.) 51.0 (7.0 gals.) 41.0 (4.7 gals.) 144.0 (17.3 gals.) 195.0 (22,4 gals.) 26.0 (3.3 gals.) 1.5 ' 100.0 5133.0 . . TIELD * One batch yield 460 gals. MIXING PROCEDURE ' m ' 1) Add water (first addition) Calgon-T, Ethylene Glycol and Advswet 33. 2) Add Atomite, Clay, Asbestos and mix for 30 minutes 3) Add the following ingredients allowing each ingredient to be * thoroughly blended before addition of the next ingredient: Resin EB-12 Emulsion RA-315 Propesol Dibutyl PhtheIste , ` , .' * '. ' 4) Add water (second addition) and AcrytoL ASS-80 (may be added, simul taneously 5) Add AMP 95 ` Biocide-290 Lehnert 10.3.01-89 SOP 0016190 August 15, 1972 Supersedes AK-502 page 2 Dated 1/28/72 '' VISCOSITY - Safer to Plant Tasting Procedure Ho. 109 Specifications: 430 to 46Qrsbender unit ,. Btabender Viscosity 430to46P Viscosity can be adjusted by addition of water, reduction of nix water, or by addition of ASE-60 in email amounts. It is bast to bold back a snail amount of water to be added if the viscosity is too high. ASE-60 nay ba added to thicken the nix should too much water have been added. Should it be necessary to add ASE-60, the pH oust again bechecked since ASE-60 la acidic and its addition will lower pH. Remember, changes in the water content affect flow properties as well as the wot density* ' WORKING CHARACTERISTICS: Shall extrude easily from tube and form a ' uniform bead chat does not sag or nrn. OPEN TIME -Refer to Plant Tasting Procedure No. 114 WRITING CHARACTERISTICSt Refer to Plant Tasting Procedure Ho. 115 TENSILE STRENGTH - Refer to Plant Testing Procedure po. 116 ALKALINITY . ," - Refer to Plant Testing Procedure Ho. 34. Adjust with small quantities of AMP Specifications: Maximum Minimum Averaea 8.3 7.7 8.0 . DENSITY Specifications; 11.00 lbs./gal 10.75 lbs ./gal 10.851ba./gal Case weight should be 35 lbs.* 1 lb. .,, ` . EDO:ala Denotes change ' r i . a, ' Lehnert 10.3.01-90 SGP 0016191 5Septanacr i t 1*72 Supersede* aa-sos Dated 8/15/72 AXROK, SEW VQAK, 2LAK7 FOEfcLA D2WALL ADHESIVE AK-302 DESCRIPTION - Drywall atud adhesive ?s&:u Tvrw I-^tarlal Function RM Soac. Percanr lit, "Itrth Water Solvent Calgor.-T Watting Agent Ethylene Otyool Solvent ' Advewet-33 Wetting Agent Aio^i:a Limestone Filler Clay 3PC3 Filler Asbestos SG210 Filler Seein B3-12 Adhesive Emulsion Elvece 1873 Adhesive Prcpcaol Fliming Agent Dibucyl Phthelate Plasticiser Water Solvent Acryeol ASE-60 Thickening Agent Al?-$5 pH Buffs? Siccide 290 Fungicide 11 182 220 217 225 12.0 0.1 3.0 0.9 27.0 9.0 0.8 8.0 30.0 1.0 C .6 2.8 3.8 0.5 0.3 617.C (74 gals.) 5.0 154.v CS.6 gala.; 46.w (5.5 gels.) 1396.2 462.3 41.0 410.0 (35 gala.) 1541.0 (173.0 gels 51.0 (7.0 gals.) 4*.3 (4,7 gals.) U4.0 (17.3'gels.] 195.0 (22.A gels.: 26.3 (1.3 gels.) 1.5 100.0 5133.0 * One batch yield 4S0 gals. ::r:-:i:sO procedure - l) Add water (first Addition) Ciilgon-T, Ethylene Glycol and Adverse 33. 3) Add Atomlte, CUy, Asbestos and mix for 30 minutes 3) Add tha following Ingredients allowing each ingredient zc be choi-oughly blond ad before addition of the next Ingredient: Hesin ES-12 Emulsion BA-315 Proposal Bibutyl Phthelate ' - ' <t) Add water (second addition) end Acrysol ASS-69 (coy be add ad caneously . 5) Add AI-2* 93 . . Bloclde-290 . ' -/ dsnofea* change . Lehnert 10J.01-91 ZDCrela * . SOP 0019193 ohm} lill ttguf lmm I * #*HV lOM^ 'W ta| fe# . Hsy 18, 19/1 8mmii4u Finull M*901 Ostof S/)/91 I HAMCTPL QgOgPTA. mwt gQlMflA few CMtttAL KIX J9 eflMwniub M-8Q1 msmmsumm Vinyl Mlci-pavpoMcoapoond tot # with pocforatad up*. to is um4 * uaiai, finishing, spotting oallhitd* JSwWttSng. U UmwiM syssiUically is sssml nln.nv pranla typo opomioot* 1258*.05 2*.0 #*2 124 aa.S p?4 300.0 faagr.iL 5000.0 fftSMAl ' . mw txm.fttf VtflcUi }U ' Cowl 9721 ,,. (polyvinyl Aleokbl) OoUa 701 (Polyvinyl Acscskn) mismi tso wta Calgon T iiHitsi 7*7*0* AitsiHS M910 . ' Men H0* Function M im>h iwm * aifliio Miitiis ia< 0.05 * i.o' JUbtiN . US , *.30 100.0 AdhulH tfaieknov 1n6o1 oO..SsOo * *200..00 Up Agent, fillo* . TttUv jbtt(<sf(US !> ABtWMSlOl 8|W 9 .. 11 . 0.25 *.25 1.73 6*00 0.05 ' 10.0 170.0 70,0 240.0. *.0 . Pill** , u _&i* 100.00 4000.0 WMH1M COOTIMBPtOIi tPfUUWHMi : M to Plan* Totting Fmoduvo 52 Hfnlwin **"<-- AvtraflO 42 16 60 infnte to rune Totting Procedure Ho. 55. Vst mt* shall ho pUffeio tad hnttary neofclog ond feed of mum on gaiety partioUs. COLOftt BBOtdU r , A' talar to-Plane- Tooting rraoadacn go. 95. Alton totpewnd bt dried, Up. shall tfoUaiaato ' when peeled beaks .. ' lifer to Plant Tasting Pvoeodaro ho. 37* Itwto shall ba no Utgn llason tracks in tho vadge sad nosy law, if say, stacks in tho chinaov .-.half of tha vadga, >- Drlsd ooapouad shosld Midi colon of standard stopla. Lehnert 10.3,01-92 * t SGP 0016207 October 3, 1972 Formula No. AK-935 NEW AKRON, NBW YORK, PUNT FORMULA ALL PURPOSE JOINT COMPOUND AK-933 DESCRIPTION OF PRODUCT - Topping Compound for topping Joints and .. spotting nailheads. FORMULA Raw Material Defoamer Mill Vanieide Asbestos 7R709 Asbestos 80210 1' Hatrosol 250 BXR Mica Calgon T Dow Resin 164 ' (XD76646) Limestone Function RM Sdc Antifoaming agent Fungicide Bulking Agent Bulking Agent Water retention aid Anticracking agent Dispersant Adhesive Filler ' 196 126 9 m 170 11 J - Percent Lb8/Baech .02 1.00 0.05 2.00 4.25 170.00 1.50 . 60.00 0.20 8.00 7.00 280.00 0.20 8.00 3.75 130.00' 83.03 3321.20 100.00 4000.00 WORKING CONSISTENCY Spa ci heat Iona.... Refer to Plant Testing Procedure No. 32. Maximum Minimum Average *" WORKING PROPERTIES Specifications 71 65 6$ Refet to plant Tasting Procedure No* 33. Wet Mix shall be plastic and buttery working and free*of grit or coarse particles. CRACK RESISTANCE Specifteations - There shall be at most only a couple of very small cracks in the wedge. ` COLOR Specifications ,,. - Neutral dried compound should match the color of standard sample. Note: For yellow compound add A lbs. of yellow oxide 2087 per batch. BD0:ee v. Lehnert 10.3.01-93 SOP 0016758 December 5, 1972 Supersedes Formula No* AK-933 Dated 20/3/72 AKRON, NEW YORK, PLANT FORMULA ALL PURPOSE JOINT COMPOUND AK-935 / DESCRIPTION OF PRODUCT - All Purpose Joint Compound for bedding, taping, and finishing Joints and spotting nallheads. FORMULA Raw Material Defoamer Mill Panicide Asbestos 7RF09 Asbestos 80210 Natrosol 250 HXR Mica Calgon T Dow Resin 164 (XD76646) Limestone ftBSS&ai RM Spec Antlfoamlng agent Fungicide Bulking Agent Bulking Agent Water retention eld Antlcracklng agent Dispersant 196 126 9 - 170 11 Adhesive Filler Percent Lbs/Batch *02 0.05 4.25 1.50 0*20 7.00 0.20 1.00 2.00 170.00 60.00 8.00 280.00 8.00 3.75 130.00 83.03 3321.20 100.00 4000.00 WORKING CONSISTENCY Specifications Refer to Plant Testing Procedure No. 32* Maximum Minimum Average 71 69 69 liiiWJvU PROPERTIES Specifications Refet to plant Testing Procedure No. 33. Wet Mix shall be plastic and buttery working end free*of grit or coarse particle*. CRACK RESISTANCE Specifications There shall be at moat only a couple of very small cracks in the wedge* ., COLOR Specifications Neutral dried compound should mateh the color of standard sample* Note: For yellow compound add 4 lbs* of yellow oxide 2087 per batch. BDOxes . -/ denotes change . Lehnert 10.3.01-94 SOP 0016759 December 5, 1972 SuperseBss Chicago Formula C-935 Dated 10/3/72 CHICAGO, ILLINOIS, PIAMT FORMULA ALL PURPOSE JOINT CCHFOOHP C-935 */ DESCRIPTION OF PRODUCT - Compound Cor taping joints and finishing Joints and spotting nalihaada. FORMULA Raw Material Function ' gfM. Soso Percent 1 Defoamer Mill Vanialie ' Antifoaming Agent 196 fungleiie 111 .02 0.05 Asbestos ZRF09 Bulking Agent 9 4.25 Asbestos S0210 Bulking Agent 1.50 Natrose1 250 HXR Water retention Aid 170 0.20 Mica Antioracking Agent - 11 7.00 Calgoo T Dispersant 0*20 Dow Resin 164 (XD76646) Adhesive 3,75 Limestone Filler 83.03 Lbs/Btcb 1.00 2.00 170.00 60.00 8.00 280.00 8.00 150.00 3321.20 WORKING CONSISTENCY 100.00 4000.00 - Refer to Plane Texting Procedure No* 32* Specifications: Maximum Minimum Average 71 65 68 WORKING PROPERTIES Refer to Plant Testing Procedure No 33* Specifications Wet Mix shall ba plastic and buttery working and free of grit or coarse particles* CRACK RESISTANCE dpaclfioatlcna There shall be at most only a couple of very smell creeks in the wedge* COLOR Specifications Neutral dried compound should match the color of atanderd sample. Note: Por yellow compound add 4 lbs. of yellow oxide 2087 per batch* SDOtels -/ denotes change i . ' Lehnert 10.3.01-95 SOP 0016789 CHICAGO, ILLINOIS PLANT FORMULA TOPPING COMPOUND C-936 torch 30. 1572 Chicago Formula 0C-936 KEW DESCRIPTION OF PRODUCT White Topping Compound Sox. copping joints end spotting naUheads* FORMULA J^aw Material Function D* loom* r; Hill Antifearning Agnet Vanlcide Fungicide * Asbestos 7RF09 Bulking Agent Asbestos SG210 , Bulking Agent Katrosol 250 KXR' Water Retention Aid Hies Aatlcracklng Agent Calgon T Dispersant Dow Resin 164 OQ76646) Adhesive Limestone Filler 196 126 9 170 um . . Percent 102 0.05 4.25 1.50 0*20 7.00 0.20 Lhs./B :.oo 2.00 170.00 60.00 8.00 260.00 8.00 2.50 100.00 100.00 jama 4000.00 WORKING CONSISTENCY Soecificatloast - Refer to Plane lastlog Procedure Ko. 32. Maximum Minimum Averece 71 65 68 WORKING PROPERTIES SPeclficatlonsT"" " r"~ . - Refer to Plant Testing Procedure No. 33. Wet Mix shall he plastic and buttery working and free of grit or coarse particles. CRACK ASSISTANCE Specifications: .. - There shell he at most only a couple of very small cracks in the wedge. COLOR Specifications} . - Neutral dried compound should match the color of standard sample# . * EDO:elx Lehnert 10.3.01-96 SOP 0018802 >>* August 23, 1972 Supersedes; Chicago formula vC-936 Dai*u Karoh 30, J972 #. CHICAGO, ILLINOIS PUKT FORMULA T0??t::n co::po,j:d c-93^ DESCRIPTION C? PRODUCT - hr.isa Topping Compound for topping joints and spotting nailhaads. FCRHTIA . Row Matorini' Function Dofoancr Mill Vanicida Antifcaning Agnat Fungicide . Asbestos 7RP09 Sulking Agent Asbestos $0210 Bulking Agent Xacrosoi 5$d HXSl - Ivxtur Ratenfioa Aii Mica Anticracking Agent Calgoa T Dow Resin 164 Dispersant . 0076646) Adhesivn ' limestone Pillar R.K. Soec, 196 126 9 170 i-i. . Porcont .02 o.os 4.25 1.50 0.20 7.00 0.20 3.75 e3.03 Lhs./I 1.00 3.00 170.00 60.00 5.00 230.60 6.CO 150.CO 3321.20 100.00 40C0.C0 utor:-:in*g consistency Soabifications: - Refer co Plane Tasting Procedure Mo. 3 2. Maxiaura Mininura Avertte 71 63 68 voa::i:;a properties Stacliicssiona: . - Refer co Plant Tasting Procedure No. 33. Wat Mix shell be plastic and buttery working &&d free of grit or coarse particles. c?ac:: resistance Specifications* There shell be at ~ost only a couple of vary snail cracks in the wedge. 00103 Specification*l Neutral dried eoapeund should natch the color of standard sample. *' SDOteln Lehnert 10.3.01-97 SGP 0016803 October 3* 1972 Supersedes Chicago C-936 Dated 8/25/72 CHICAGO, ILLINOIS, PLANT FORMULA TOPPING COMPCWND C-936 DESCRIPTION OF PRODUCT - White Topping Compound for topping joints end spotting nailheads. -/ FORMULA Raw Material Function $1 Spec, Percent Lbs/Batch Deafoamer Mill Vanicide Aebeatos 7RF09 , Asbestos SG210 * Natrosol 250 HX& Mice Calgon T * Dow Resin 164 (XD76646) Limestone Antifoaraing Agent Fungicide Bulking .Agent Bulking Agent Water Retention Aid Anticracking agent Dispersant Adhesive Filler 196 126 9 170 11 m .02 0.05 4.25 1.50 0.20 7.00 0.20 L.00 2,03 170.00 60.00 3.00 280.00 8.00 3.125 125.03 83.655 334<-. 23 100.00 4300.00 WORKING CONSISTENCY Specifications - Refer to plant testing procedure no. 32. Maximum Minimum A'vera urn 71 65 68 WORKING PROPERTIES Specifications - Refer to Plant Testing Procedure Ko. 23. Wee Mix shall be plastic and buttery working and free of grit or coarse particles. CRACK RESISTANCE Specifications - There shall be at most only a couple of very snail cracks in the wedge. COLOR Specifications . - Neutral dried compound ahould match the color of standard sample. -/ denotes change - EDO'.els * Lehnert 10.3.01-98 SOP 0016804 October 3, 1972 . Supersedes Akron Formula 0AK*936 Dated 3/30/72 AKRON, NEW YORK PLANT FORMULA TOPPING COMPOUND AK-936 , DESCRIPTION OF PRODUCT - White Topping Compound for topping joints end spotting nallheads. ` -/ FORMULA. . SSfMSx Vanicide . Asbestos 7RF09 Asbestos 8G210 Netrosol 230 QKR Mica Calgon T Dow Raeln 164 (ED76646) Limestone Function Antlfoemlng Agnet Fungicide Bulking Agent Sulking Agent Veter Retention Aid Antloreoking Agent Dispersant , m Adhesive Filler Mi flpq,ep. . 196 , 126 9. .- ` 170 11. m' *Sa \020 0.050 4.250 l.30o 0.200 7.000 0.200 3.123 84.695 100.00 1.00 2.00 170.00 60.00 8.00 280.00 8.00 125.00 3346.20 4000.00 . WORKING CONSISTENCY Specifications: - Refer to Plant Testing Procedure No. 32. Maximum Minimum Average 71 63 68. . WORKING PROPERTIES Soeolficatlongt " ' CRACK RESISTANCE Specifications t . - Refer to Plant Testing Procedure No. 33. . '' ' ' Wet Mix shell be plketls and buttery working and free . of grit or coarse partlolea. .: * ` ** .. There shell be et most only a couple of vary small * " cracks In tha wedge. . '- COLOR Specifications: * * .. - Neutral dried compound should match tha color of < standard sample. . BDOela -/ denotee change Lehnert 10.3.01-99 SOP 0010796 AKRON, NEW YORK PLANT FORMULA BEDDING" COMPOUND AK-937----- March 30, 1972 Akron Formula lAK-937 NEW ' DESCRIPTION OP PRODUCT * White Bedding Compound for bedding Joints. FORMULA ]Raw Material' Function Defoeaer/Min Ant learning Agnec Vanieide Fungicide * Asbestos 7RF09 Bulking Agent Asbestos SG210 ,,Bulking Agent Netrosol 250 BKR * Water Retention Aid Mice Anticracking Agent Calgort T Dispersant Dow Resin 164 (XD76646) Adhesive Limestone Filler R.M. Sooc. 196 * 126 9 -* 170 U. m Percent 102 0.05 4.25 1.50 0.20 7.00 0.20 3.00 83.78 '' 100.00 Lbs./S 1.00 2.00 170.00 60.00 8.00 280.00 8.00 120.00 4000.00 WORKING CONSISTENCY Soeclflcatlons: . - Refer to Plant Testing Procedure No. 32. Maximum Minimum Ay*bs 71 65 . 68 WORKING PROPERTIES Specifications: Refer to Pleat Testing Procedure No. 33. Wet Mix shell be plastic and buttery working end free of grit or coarse particles. CRACK ASSISTANCE Specification!: There shall be at moat only e couple of very small crack# la the wedge. COLOR Specificationst - Neutral dried compound ahould match the color of eteaderd4 sample. t . EDOxels tehnert IOAoWm SGP 0016812 AKRON, NEW YORK PLANT FORMULA BEDDTWr COMPOUND AK-937 July 27, 1972 , Akron Formula fAK-937 Supersodea formula dated 3/30/72 DESCRIPTION OF PRODUCT - White Bedding Compound for bedding. Joints. Raw Material' Function Dafoamor.'MlII Antifoaming Agnet Vanieide Fungicide * Asbestos 7RF09 Bulking Agent * Asbestos SG210 ' .Bulking Agent Natrosol 250 HXR - ' Water Retention Aid Mica Antloracklng Agent Calgon T Dispersant Dow Resin 16V <KD7664fc> Adhesive Limestone Filler . R.M. Soec. Percept 196 i02 126 0,05 9 4.25 m 1.50 170 ' U, 0*20 7.00 0.20 3.75 -11x53 100.00 Lbs./3 1.00 2.00 170,00 60.00 8,00 280,00 t 8,00 150,00 3321.20. 4000.00 WORKING CONSISTENCY * Boecifichtionss ' WORKING PROPERTIES Scsciflcations t - Refer to Plant Testing Procedure No, ;32. Maximum Minimum Avarsea 71 6$ 63 Refer to!Plane Testing Procedure No, 33. Wee Mix shall be plistie end buttery working and free of grit or coarse particles. CRACK RESISTANCE Specifications * There shall ba at nose only a couple of vary snail cracks in eha wedge* CObOR Specifications: Neutral dried . compound should match the color of standard sample, # . EDO:ale Lehnert 10.3.01-101 SOP 0016813 October 3, 1972 Supersedes AK-937 Dated 7/27/72 AKRON, NEW YORK, PLANT FORMULA BEPDIHQ COMPOUND AK-937 DESCRIPTION OP PRODUCT - White Bedding Compound for bedding joints. / wsm Raw Material Defearner MIX! Vanicide Asbestos 7BP09 Asbestos 8G210 Natrosol 250 BXR Mica Calgon T Dow Resin 164 (XD76646) Limestone Function sum Percent Lbs/Batch Antifoaming Agent Fungicide Bulking Agent Bulking Agent * Water retention eld * Antioracking agent Dispersant. 196 126 9 . ep ' 170 11 m .02 . 0.03 4.25 1.50 0.20 7.00 0.20 1.00 2.00 170.00 60.00 8.00 280.00 8.00 Adhesive Filler 4.375 175.00 82.405 3296.20 100.00 4000.00 WORKING CONSISTENCY Specifications ' Refer to Plant Testing Procedure No* 32* Maximum Minimum- Average 71 65 68 WORKING PROPSBTXBB Specifications CRACK RESISTANCE Spec iilcatIons Specifications Refer to Plant Testing Procedure No. 33. Wet Mix shall be plastic and buttery working and free of grit or coarse particles. ' There shall be at most only a couple of very small cracks In the wedge. Neutral dried compound should match the color of standard sample. - -/ denotes-change EDOtele Lehnert 10.3.01-102 SGP 0016814 f\ VuV) i ' CHICAGO ILLINOIS PLANT FORMULA. BEDDING COMPOUND C-937 March 30, 1972 Chicago Foraula 00-937. NEW . ' * * DESCRIPTION OF PRCDCCT - WhitO godding Coopound for bedding Jaintta. Raw Material Oa^oaiwr.'MIII Venlcide Asbaetot 7SF09 Aabeeeoa 80210 ' Xatroaol 330 BXft * Mica Balgoa T Dou Reain 164 (XD76646) Lifeatone function Antlfoaiaing Agnee Fungioida ' Sulking Agent Bulking Agent Hater Retention Aid Anticracking Aganc Diaparaanc R.H^Swo,. 196 126 9 - 170 . 11 " Percent v02 . 0.03 4.25 1.50 0,20 7.00 0\ .20 Adbeeiva Fillar 3.00 ' ' JM 100.00 Lba.Zlaech 1.00 2.00 170.CO . i0eC3 6.00 280.00 ' * 8.00 120.00 3351.20 4000.00..,. . WORKIKO CONSISTENCY ..SoaoiiiBOtigML *. Refer CO PUttC Teeting Procedure Ho. 32. Kwcinwm IflajfflB ASUSOI 71 65 68 WORKING PROPERTIES Sneaidlcaclana! ftaftr to Plant Toiling Procedure So* 33. Hot Kix thall be plaaele and buttery working and 2raa of grit or coaree particle*. CRACK RESISTANCE SpeclficAtioaat . - Thera ahell ha ae coat only a couple of vary eaall crack* to the wedge. COLOR Specification*t ' - Neutral dried compound thou1<S natch die color of ataadard ample. EDO:els 8QP 0016817 Lehnert 10.3.01403 JUiy-27, 1972 . Supersedes Chlcano <>937 Dated 3/30/7^ CHICAGO ILLINOIS PLANT FORMULA BEDDING COMPOUND C-937 DESCRIPTION OP PRODUCT - White Sodding Compound for bedding Joints. FORMULA Saw Material' Defoaaer. Kill Vanlcide Asbestos 7RF09 Asbestos SG210 Katrosol 250 HXR Mica Calgon T Dow Resin 164 (XD76646) Limestone Function Antljfoomlng Agnet Fungicide Bulking Agent Bulking Agent Water Retention Aid Anticracking Agent Dispersant Adhesive Filler R.M. Spec* 196 126 9' m 170 n, as Percent .02 0.05 4.25 1.50 0.20 7,00 0.20 Lbs./Bate l.CO 2.00 170.00 60.00 8.00 280.00 8*00 3.75 SM1 100.00 150.00 3321.20__ 4000.00..... WORKING CONSISTENCY specificationsi .- m WORKING PROPERTIES Specifications* - Refer to Plant Tasting Procedure No. 32. Maximum Minimum Average 71 65 68 Refer to Plant Tasting Procedure So* 33. ,. Wee Mix shall be plastic and buttery working and free ' of grit or coarse particles. CRACK RESISTANCE Specificationsi There shall be ae most only a couple of very saall cracks in tha wedge. COLOR Specifications t ,. - Neutral dried coapound should natch tha color of standard sample* . EDOtela Lehnert 10.3.01-104 SOP 0016818 April 20. 197? TsI-943 NOT FOHMDLA ACWDPSCO, T.TYEaX'TAYSKBPHBUNCTglLFDOtHCHtUTUtaKmOW. 8T(8PXlt-l9M4n3) FORHOIAl na Material Function B.M. Span. Percent Lba/Batoh Gypsum Staramio Stroh,747 Hamico Starch 267 Titanium Dioxide BAAS Papered . Tiller Adhoeive Adhesive Pigment Wgen|p 221 222 .624 1.220 2e 440 2.440 4.690 7100 100 200 200 400 Triton 1120 * . ' Vanioide (l)Asbeatos S0210 , Wetting . oId0 Thickener 0 Cl :$t - * 2.196 100.000 8 6 1*0 3196 (1) Hotel This formula may be made by using TBX-942 and adding the proper amount of Asbestos 8Q210 to the. texture mixer.^ WORKING CONSISTENCY! Refer to Plant Testing. Prooedur*. No. Mix 0 90 water/DM and allow to stain IS minutest then check Brabender vii * vf BRABBNPER tmiTSi Minimum 60 Maximum 120 100 BOND I 5FE0lPICATI0Nt Test Procedure No. 35# , .^ * ' Tape shall show at least a 50^ fiber tear when dry. CRACK RESISTANCE!, SPECIFICATION:----COLOR} . ' SPECIFICATION! Test Procedure No. 37* ^ ` There shall be no large fissure crack. White # * '` Dried compound snail match color of standard sample. VAfllQIDg 8fOX T58I? STARCH SPOT TBSTi Teet Procedure No. 67* Test Procedure No. 112. ' Lehnert 10.3.01-105 QWQidek SGP0016924 April 13, 1973 TEX-943 Supersedes Formula TEX-943 Dated April 20, 1972 ACME, TEXAS PUNT FORMULA NO* TEX-943 POLYSTYRENE CEILING TEXTURE (PRE-MIX) FORMULA Raw Material Oypsum Staramie 747 Kamico 267 T102-RA4 Paparad Attagel 40 Vanlcide Function R.M. Spec. Filler Adhesive Adhesive Pigment Pigment Thicks 192 23 221 222 Percent Lbs/Batch 63.555 1.211 2.422 1.816 6900 100 200 150 400 ' ^ . a#* 9 WORKING CONSISTENCY - Refer to Plant Testing Procedure No. 109* Mix 0 90 water/DM and allow to stand for 15 minutes, then check Brabender visoosity. BRABENDER UNITS BOND specificationi - Minimum 80 Maximum 120 Average 100 - Test Procedure No. 35 Tape shall show at least a 50J& fiber tear when dry. 1 CRACK RESISTANCE specifications Test Procedure No. 37 There shall be no large fissure eraok. COLOR * ' specifications -White Dried compound shall match color of standard sample; VANICIDB SPOT TEST - Test Procedure No. 67 STARCH SPOT TEST - Teat Procedure No, 112 mig Lehnert 10.3.01-106 SGP 0018925 /' K-U.I- July 22. 1976 Supersedes Formula T8X-943 Dated 4/19/73 ACME, TEXAS PLANT FORMULA NO. TEX-943 POLYSTYRENE CE1LINQ TEXTURE (PRE-MIX) -/ FORMULA ti&w Material Function RM Spec Percent' Lbs/Batch Gypsum Stararalc 747 Hamico 2o7 T102 Papered . Attagel 40 Vanoide Oellufloc DB 33 G&l&ptosol 413V Filler . Adhesive Adhesive Pigment Flfloent ' Thickener Fungicide Bulging agent Thickener 192 23 221 222 9 126 223 96.425 1.209 2.419 1.813 4.935 1.813 .097 1.209 .191 7150 100 200 150 400 150 9 100 1ft f 100,000 9273 WORKING CONSISTENCY - Refer to Plant Testing Procedure No. 109. Mix <9 90 water/DM and allow to stand for 1? minutes, then check Brabender viscosity. BRABBND3R UNITS - Mininun Maximum Average 90 120 100 * BOND ' specif1oations - Test Procedure Ho. 35 Tape shall show at least a 50 fiber tear when dry. CRACK RESISTANCE - Test Procedure No. 37 Specifications There shall be no large fissure crack. COLOR Specifications - White .* Dried compound shall match color of standard sample. VANCIDS SPOT TEST - Test Procedure No. 67 STARCH SPOT TEST - Test Procedure Ho. 112 GWQiJg \ Lehnert 10.3.01-107 S *. , SOP 0016920 October 22,1976 Supersedes Formula TEX-943 Dated 7/22/76 ACME, TEXAS PLANT FORMULA NO* TRX-943 POLYSTYRENE CBILINQ TBXTURE (FRE-MIXl FORMULA Haw Material Funation RM Spec Percent Lbs/Batch Ovpsum 3taramie 747 Haraico 267 T102 Paperad Attagel 40 Vancide Cellufloo DB 33 / Cendtlv 4928 WORKING CONSISTENCY Filler Adhesive Adhesive Pigment Pigment * Thickener Fungicide Bulking agent Thickener 192 23 221 222 8 126 223 06.425 1*209 2,41o 1.813 4.635 1.613 .097 1.209 .181 7150 100 200 150 400 150 6 100 IS 100.000 8273 Refer to Plant Testing Procedure No. 109. Mix $ 90 water/DM and allow to stand for 13 minutes, then check Brabender viscosity* BRABKNDBR UNITS - Minimum Maximum Average . ' ` SO 120 100 BOND Specification 1 - Test Procedure No* 35 Tape shall show at least a 50# fiber tear when dry* CRACK RESISTANCE Specification: COLOR ""Specification; Test Procedure No. 37 There shall be no large fissure crack. - White Dried compound stall match color of standard sample* VANOIPg SPOT TEST - Teat Procedure No* 67 STARCH SPOT TEST - Test Procedure No. 112 GWOijg Lehnert 10.3.01-108 SGP 0010927 . I rO I ! November 7, 1C72 Supersedes Formula 7SZ-&J.2 Dated 7/1/71 ACE, TEXAS l>LAt?Y FORrWU ' G-P TEXTURE HOK-AOORECATEP NO. TEX-9M DESCRIPTION OF PRODUCT - A dry pothered produot, containing no aggregate, for mixing with water to produce textured finishes on gypsum wallboard by means of spraying, rolling, or troweling. -/ FORMULA g RAW MATERIAL FUNCTION R.M. SPEC # PgRCEirr LB/3ATCH TEX-25 RS627SC Hamico 267 Paperad Ti02 - RA4fc Asbestos SG210 Vancide Triton X120 Filler Adhesive Adhesive Pigment Extender Pigment Fiber Filler Fungicide Wetting Agent 162 222 221 126 da.3125 1.5425 2.5 3.75 1.875 1.S75 .0625 .0625 100.0 7065 125 200 300 150 150 5 _JL 8000 SPECIFICATIONS8 WORKING CONSISTENCY - Mix at 90 W/P. Allow to soak for 10 minutes. -/ Brabender Number t WORKING PROPERTIES Maximum Minimum Average 120 SO 100 - Refer to Plant Testing Procedure-No. 13. Material shall be plastic, and free from any coarse, gritty or undispersed particle. Material shall be free from lumps due to incomplete mixing. * BONDING PROPERTIES - Refer to Plant Testing Procedure No. 35* After compound has dried tape shall show at least 50# fiber tear when delaminated. CRACK RESISTANCE - Refer to Plant Testing Procedure No, 37. There shall be no large fissure cracks in the wedge and no cracks in the thinner half. COLOR VAKICIPE SPOT TEST STARCH SPOT TEST - Whites Color shall match standard sample. - Plant Test Procedure No. 68. - plant Test Procedure No. 112. ED0:ct /Denotes change in reissue. Lehnert 10.3.01-109 SGP 0016940 * S-3-7Z. April 14/ 19TT Supersedes Formula Ho. TBX-952 Doted 11/17/71 r? ACME. TEXAS PLANT FORMULA ALL PURPOSE JOINT COMPOUND, FORMULA NO. TEX DESCRIPTION OF PRODUCTi - - All Purpose compound for taping and finishing joints, spotting nsllhsada and texturing. / FORMULAS Function hfes/Patch Gendriv 4928 Thlcknet 223 0.30 24.00 Vaniclde 512 Fungicide * Calvatol 6278<L ^ , Adhesive 126 0.05 4.00 126 1.75 140,00 Reiser -Wlpa dZa^4./ Adhesive 161 1.00 80.00 . Asbestos && S CJ td Fibpr Filler 9 7.09 32VC00 * Mica p80-H Anti-Craoking Agent n 5.00 400.00 Defoamsr MU7 , Anti-Foaming Agent * 0.10 8.00 Land Plaster TEX-25 Filler . * 84,80 iMfcOO? 100.00 8000.00 WORKING CONSISTENCY: Specifications: WORKING PROPERTIES; Specifications BONDING PROPERTIESt Specifications CRACK RESISTANCE COLOR: Specifications - Refer to Plant Testing Procedure No. 32. Maximum Minimum Average 62 58 60 Refer to Plant Testing Procedure No. 33. Wet nix shall be plastic and buttery working and free of grit os coarse partiales. Refer to Plant Tasting Procedure No. 35. After compound has dried, tape shall delaminate when peeled back. ' There shall be at most only s couple of very small cracks in the wedge. White ' Dried compound shall not vary in dolor from preceding batches. ' Lehnert 103.01-110 / Denotes change in this reissue. EDOtdek SGF 0017203 JX_u\ I March II, 1974 Haw Formula No. TEX-933 ACME, TEXAS, PLANT FORMULA ALL PURPOSE JOINT COMPOUND FORMULA NO. TBX-953 .ISCRIFTIOB OF PRODUCT All Purpose compound for taping and finishing Joints, spotting nallheads and texturing. To be shipped to Mctnpble only. FOMJLA Function BM Soso Parent Lbfl/gal Cendriv 4928 Thlckner 223 Vanicide 51Z Fungicide 126 Gelvatol 6000 Adhesive 126 Aetdgel 40 Fiber Filler 161 Asbestos SO 210 ` Fiber Filler 9 Mica p80-H Anticracking agent 11 Oefoamer Mil7 Antifoamlng agent . -- Land Plaster TEX-25 Filler -- 0.30 0.03 1.73 1.00 2.50 5.00 0.10 89.30 24.00 4.00 140.00 80.00 200.00 400.00 8.00 7244.00 100.00 8000.00 WORKING CONSISTENCY Specifications: -Refer to Plant Testing Procedure No. 32. Maximum Minimum Average 62 sa 60* WORKING PROPERTIES Specifications - Refer to Plant Testing Procedure No; 33. Wet nix shall be plastic and buttery working and free of grit or coarse partloles, BONDING PROPERTIES Specifications - Refer to Fleet Tasting Procedure No. 35. After compound has dried, tape shall delaminate when pooled back. CRACK RESISTANCE - There shall be at most only a couple of very small cracks in the wedge. COLOR Specifications White Dried compound shall not vary in color from proceeding batches. NOTE; For yellow compound, add 4 lbs. of yellow oxide. WNGtele Lehnert J 03,01-111 3GP 0017204 fV \w December 16, 1975 Supersedes formula TBX-953 Dated 3/11/74 ACME!, TEXAS, PLANT FORMULA ALL PURPOSE JOINT COMPOUND FORMULA NO. TBX-9S3 DESCRIPTION OF PRODUCT - All Purpose compound for raping end finishing Joints, spotting nailheads end texturing, To be shipped to Memphis only* -/formula Sorbitol Cenclrlv 492$ Venloide S1Z Gelvatol 6000 At tagsL AO Asbestos SO 210 Mica p80-H Defosmer M117 land Plaster TEX-25 Function RM Spec Boron Stabilizer -- Thiekner 223 Fungicide 126 Adhesive 126 Fiber Filler 161 Fiber Filler 9 Anticracking agent 11 Antlfoamlng agent -- Filler - Percent .50 0.30 0.03 1.73 1.00 2.SO 3.00 0.10 68.8 Lba/Batch 40.00 24.00 4.00 140.00 80.00 200.00 400.00 8,00 r> i* J>ET G6 . 1*0 710L0 n% 100.00 8000.00 -cvc*fi WORKING CONSISTENCY Specifications: - Refer to Plant Testing Procedure No* 32, Maximum Minimum Average 62 38 60 WORKING PROPERTIES Specificstions Refer to Plant Testing Procedure No. 33. Wet mix shall be plastic and buttery working end free of grit or coarse particles. BONDING PROPERTIES Specifications Refer to Plant Testing Procedure No. 35. After compound has dried, tape shall delaminate when peeled back. CRACK RESISTANCE Thera shall be at most only a couple of very small cracks in the wedge. COLOR Specifications White . Dried compound shall not very in color from proceeding batches. . NOTE: For yellow compound, add 4 lbs. of yellow oxide. -/ denotes ohange WNGsjg 10.3.01-11* SGP 0017205 June 29, 1971 Supersedes Formula TKX-991 Dated 5/27/70 mim SPSSD SET JOINT COMFOUMP WHnKJEEX-991 (60 minutes and 2 hour working cement) DESCRIPTION OP PRODUCT: . - For use in reinforcing and conceding Joints and nallheads. . ' / FORMULA; Raw Material Function R. M. Soso. toSSER Sodium Citrate Notrosol 230HXR Gelvatol RS-6278C Oelvc CF702 Asbestos 80210 Asbestos 7RP09 Mica p80H Defoemor Mill Vanielda TEX-38 Retarder 134 Thickoer 170 Adhesive 162 Adhesive 167 Fiber Filler SB Fiber Filler 9 Anti-Cracking Agent 11 Anti-Foaming Agent 196 Fungicide 126 Plaster - | 0.10 0.20 2.2S ' 0.50 0.50 2.23 4.00 0.05 0.05 90.10 100.00 Adjust quantit/ according to set time requirements. 0.750 1.500 16.873 3.750 3.730 16.875 30.000 0.375 0.375 675.730 750.000 W0RK1BC CONSISTENCY: Specifications - * Refer to Plant Testing Procedure No. 32. Minimum Average 62 58 - 60 SETTING TIME; Specifications - Refer to Plant Testing Procedure Mo. 6 (slow set) lliflfam Average 110 mins. 3% hours 70 mine. 2k hours 90 mins. 3 hours ' WORKING PROPERTIESi Specifications BONDING PROPERTIESt Specifications CRACK RESISTANCE; Specifications - Refer to Plant Testing Procedure Mo. 33. Muse be plsstia and buttery working( free of grit or coarse particles. - Refer to Plant Testing Procedure Mo. 35. After compound has dried, tape shall doldmlnate when peeled back. - Refer to Plant Testing Procedure No. 37. There shall be no large fissure cracks in the wedge and very foe, if any, cracks in the thinner half of the wedge. -/ Denotes change In this reissue. EDO: dele Lehnert 10.3.01-113 SGP 0018387 September 7, 1971 Supersedes Formula TEX-991 Dated 6/29/71 ACME. TEXAS PUNT FORMULA SPEED SET JOIST COMPOUND WHITE TBX-9M (2 hour working cement) . DESCRIPTION OF PRODUCT - For uae In reinforcing and coocelling Joints and oallheflde* . -/ Raa Matgyifll gtf.np^on R.H. Spec* JESJSLSal *Sodium Citrate Natrosol 250 HXR Gelvatol R8-6278C Gelva GP702 Asbestos SG210 Asbestos 7RF09 Mica p80U Defoamer Ml 17 Vanicidc Denacal Retarder Thickner Adhesive Adhesive Fiber Filler Fiber Filler Anti-Cracking Agent Anti-Foaming Agent Fungicide Plaster 134 170 162 167 - 9 11 196 126 0.10 0.750 0.23 2.00 U875 15.000 O.SO 1.50 3.750 11.250 3.23 24..37S 5.00 37.500 .10 .750 MM- .730 6457375 * 100.00 750,000 *Adjuae quantity according to set time requirements. WORKING CONSISTENCY8 Specifications - Refer to Plant Testing Procedure No. 32* Maximum Minimum Average 62 58 60 ~f SETTING TIME! Specifications Refer to Plant Testing Procedure No. 6 (slow set) 2k hours 2% hours 3 hours ttORKIHO. PROPERTIES t Specifications Refer to Plane Testing Procedure No. 33. Muse be plaatic and buttery working; free of grit or coarse particles* BONDING PROPERTIES! Specifications Refer to Plant Testing Procedure No. 35* After compound has dried, tape ahall delaminate when peeldd back. S^OgsJSMpj; Specifications Refer to Plane Testing Procedure No. 37* ' There shall ba no large fissure cracks in tha wedge and very few, if`any, arafcks in tha thinner half of the wedge* Lehneri 10,3.01-114 -/ Denotes change in this reissue. BDOsdek ., * * . ` . ' . SOP 0018363 .' I .' . I...................................................... .................... i : ' . ... -- . ' h-V\C> ' February It, 1972 Supersedes ` formula TEX-991 Dated 9/7/71 ACHg. TEXAS PLANT FORMULA SPESD SET JOINT COMPOUND WHITE TBX-991 (2 Hour Working Cement) 9-2(- 7 C, </ 2 DESCRIPTION OF PftOOUCT - For use in reinforcing and conceiting Joints end nallheada. * FORMULA lJ:iw Mntarl at RupeeJon ^HlSOC . Percent tbs/Batch *3odium Citrate Natrosol 260 ItXR Cclvatol RS-6273C Colvs GP702 , Asbestos 8G210 * Asbestos 7RF09 Mica p80H Dafoauer Mill Vsnicide Denscal Retarder * . 134 , Thlckn'er Adhesive Adhesiva ` Fiber filler ' 170 162 167 MS Fiber Filler Anei-Crsoklng agent Aatl-Ppenlng agent i: Fungicide Plaster 9 11 196 126 - . .* *Adjuse quantity according to act tine .requirements. 0.10 0.23 l.SO * 0.30 1 . 1.75 5.00 ` 3,00 . .10 as..1700 100.00 . 0.750 1.875 11.250 3.750 13.123 37.300 37.300 .750 .750 -M*.750 750.000 ' WORKINfl CONSISTENCY Specifications - Refer to Plant Testing Procedure no* 32* Maximum Minimum Average _ SETTING TIME Specifications WORKING PROPgRTtES Specifications -90sane PROPgRTtES SpnWlQQd CRACK RESISTANCE Specifications 62 , '58 60 Refer to Plant Tasting Procedure Ho. $ (slow set) 3fc hours 2^ hours 3 hours Refer to Plsnt Testing Procedure No. 33. Must be plastic and buttery working; free of grit or ooarse particles. a Refer to Plant Testing Procedure No. 33. After cowsund ha* tape altall delaminate when peeled back. *- ' Refer to Plant Testing Procedure No. 37. There ahs'll be no large fisaure cracks in the - wedge end very few, if any, cracks In the thinner half of the wedge. -/ Denotes change in this reissue. Lehnert 10.3.01-115 SGP 0018369 JUh* J} eu.y 2& f-//** '4*i*s*a**- #*3-&**?? September 8, 1971 HEW FORMULA TBX-992 ACHB. TEXAS PLANT FORMULA 8PBBD 3BT JOINT COMPOUND WHITE TEX-992 (1 hour working cement) DESCRIPTION OF. PRODUCT! - For use in reinforcing and cancelling joints end nallheeda FORMULA* Raw Material Function R.M. Spec. Percent Lbs/Batch *9odium Citrate Natrosol 250 HXR Galvacol RS-6278C Gslva GP702 Asbestos SG210 Asbestos 7RF09 Mica pSOit Defoamer Milt Vanlcide Denscal Retarder Thickner ' Adhesive Adhesive Fiber Filler Fiber Filler Anti-Cracking Agent Anti-Foaming Agent Fungicide Plaster 134 0.10 0.750 170 0.25 1.875 162 2.00 15*000 167 0.50 3.750 m 1.50 11.250 9 3.23 24.375 11 5.00 37.500 196 10 .750 126 .10 .750 as $7.10WtOS*' .645.375* 4 100.06 730.000 *Adjust quantity according to set time requirements* WORKING nonaiSTBNCYi Specifications Refer to Plant Testing Procedure No. 32. Maximum Minimum Average 62 58 60 SETTING TIME: Specifications Refer to Plant Testing Procedure No* 6 (slow set) 110 min. 70 min. 90 min. WORKING 'PROPERTIESs Specifications Refer to Plant Testing Procedure No. 33. Must be plastic and buttery working; free of grit or coarse particles. BONDING PROPERTIES* Specifications Refer to Plant Testing Procedure No. 35. ' ` After compound has dried, tape shall delaminate when peeled beck. * ,* CRACK RESISTANCES Specif!eations Refer to Plant Testln g. Procedure No. 37. ' There shall be no largd-fissure eraoks in the wedge and very few, if'any, eraoks in the thinner half of the wedge. . * * Lehnert KU.Ol-Htf EDOidek SOP 0018376 January 28! 1972 Supersede? TEX-992 Dated 9/8/71 ACMB. TBXA8 PtANT FORMULA SPEED SET JOINT COMPOUND WHITS TEX-992 (1 hour working cement) DESCRIPTION OF PRODUCT} ~ For use in reinforcing and cancelling joints and nailheads. MUM: Raw Mucur lal Punctloq RfMr Spec. Percent *Sodlum Citrate Hotrosol 250 HXR Golvatol RS-6278C Colva CP702 Asbestos So210 Asbeatoa 7RP09 Mica p80H Dofearner Mill Vanlcide Densest . .q Retarder THleknce Adhesive Adhesive Fiber Filler Fiber Filler ' Anti-Cracking Agent Antl-Foemlng Agent Fungicide Plaster 134 170 162 167 as 9 11 196 126 10 *Adjust quantity according to set time requirements, 0.10 0.750 0,25 1.50 1.873 tStr* 11.250 " 0,30 3,750 & '* . 1.73 13.123/ * * * 5.00 37.500 3? ** 3.00 37.300 > a r* .10 *750 * 4- ,10 .750 ' . 83.70 100.00 750.000 WORKING CONSISTKNCY'i Spot iflenttone - Refer to Plant Testing Procedure Ho* 32. Maximum Minimum Average SETTING TIMEi Specifications 62 $6 60 Refer to Plant Testing Procedure Ho* 6 (slow set) 110 tain. 70 min* 90 min. WORKING PROPERTIES! Specifications Refer to Plant Testing Procedure Ho. 33. Must be plastic and buttery workings free of grit or coarse particles. BONDING PROPERTIES* Specifications Refer to Plant Testing Procedure No* 35* After compound has dried, tape aha11 delaminate when peeled back* . CRACK RBSIBTAHC81 Specifications Refer to Plane Teatin g Procedure Ho. 37* ' There shell bo no large. fiseure cracks in the vodge and very few. If any, craqk* in the thinner half of the wedge* -/ denotes change EDOtals Lehnert 10.3.01-117 SGP 0018377 A vu June 29, 1971 Supersedes Formula 993 Dated 2/27/70 ACME. TEXAS PLANT FORMULA 3PBBD SET JOINT COMPOUND (YpthOWl TEX-993 (60 minute and 2 hour working cement) PUSOtOPTXOH OF product? - For use in reinforcing and conceillng joints and nailhead** / FORMULA: Raw Material YdllowOxida Function Figment R. M. Spec. 138 ^Sodium Citrate Recorder 134 Nstvoaol 2S0KXR Thicknor 170 Gelvatol U8-6278C Adhesive 162 Gelva GP702 Ashes tua SG210 Asbestos 7RF09 Adhesive Flbor Fillor Fiber Filler 167 - 9 Mien p80l( Anti-Cracking Agent U Defoamcr Hill Anti-Foaming Agent 196 Vaniuido Pungioide 126 TEX-38 Plaster ^'Adjust quantity according to set time requirements. Paraant 0.20 0.10 0.20 2.25 ' 0.50 0.50 2.23 4.00 0.05 0.05 100.00 Lhs/Bttch 1.500 0.750 1.500 16.875 3.750 3.750 16.873 30.000 0.375 0.375 -M / WORKIffl? CONSISTENCYs Specifications Refer to Plant Testing Procedure No, 32. Maximum Mf.nimuip Average 62 58 60 SETTING TIMBs Specifications - Refer to Plant Testing Procedure No, 6 (slow set) Maximum Mlnlauq Average WORKING PROPERTIESt Specifications 110 mins. 3*:t 4- 3% hours 70 mins. hours 90 mins. 3 hours - Refer to Plant Testing Procedure Ho.33. Must he plastic and hueter/ working; free of grit or ooasse particles. BONDING PROPERTIES; . Specifications - Refer to Plant Testing Proceduro No. 35. Aftar compound has dried, tape shall delaminate when peeled back. CRACK RESISTANCEi Specifications - Refer to Plant Testing Procedure No. 37. Thare shall be no large fissure oracks In Che wedge and very few, if any, cracks to the thinner half of the wedge. . -/ Doootes change in $hia reissue. ,, _ ft1 .4Q X<sbn**il03, EDO? dek SGP 0018380 January 28, 1972 * Supersedes TEX-993 Oared 9/8/71 ACliZ. TSXAS FLAHT E-ORHMA SPEED SBT JOINT COMPOUND WHITE TEX-995 (k hour working cement) nssc>UTPTTQM OP PRODUCT! - For use in reinforcing and conoelllng Joints end nal-lheads. . vomuu Rnw Materiel Function SJLJ&ssl- *Sodiuu Cl eveto Nocroeol 250 HXR Oelvatol RS-62780 Golve GP702 Asbestos SG210 Asbestos 7RFQ9 Mice p80K flefoawor Mill Vanioide Denscal '. Retarder Thickner Adhesive Adhesive Fiber Filler Fiber Fillec Anti-Cracking Agent Anti-Foaming Agent Fungicide Plaster . 134 170 162 167 m 9 11 196 126 *Adjust quantity according to set time requirements* Percent Lbs/Batch 0.10 0.25 1.50 0.50 . 1.75 3.00 5.00 .10 .10 65.70 iSoToo 0.750 1*675 11.250 3*750 13.125 37*500 37.500 *750 .750 642.750 750.000 WORKING CONSISTENCY) Specifications - Refer to Plant Testing Procedure No. 32. Max input} Minimum} Average 62 58 60 SETTING TIME: . - Refer to Plant Tasting Procedure No. 6 (alow set) Specifications 90 min. 40 min* 60 min* WORKING PROPERTIES; Specifications - Refer to Plant Tasting Procedure No. 33. Must be plastic and buttery working} free of grit or coarse'particles* , BONDING PROPERTIESiSpecifications - Refor to Plant Testing Procedure No* 33* . After qompqurol h dried, deiwinRft when peeled back* CRACK RESISTANCE! Spec ifleal; ions Refer to Plant Testing Procedure No* 37. There shell be no large fissure ppseks in the wedge and very few, if any, cracks in the thinner half of the wedge* Lehneft 10*3,01419 7-7-3 -/ denotes change EDO:sis SGP 0018407 k -Uo September 8, 1971 NEW FORMULA TEX*999 ACME. TEXAS PLANT FORMULA . SPEED SET JOINT COMPOUND WHITE TBX-995 (V hour working cement) DESCRIPTION OF PRODUCTi For use in reinforcing and coneeiUng joints end nailheads. Raw Material Sodium Citrate Natrosol 250 HXR Golva tot RS-62760 Gelva GP702 Aabeatos SG210 Asbestos 7RF09 Mioa p80H Defoaoter Mill Vanicide 4 Densea1 - Function JLKt-SRSa- Percent Lbs/ Batch Retarder Title knot ,,. Adhesive Adhesive * Fiber Filler Fiber Filler . 4nt 1-Cracking Agent Anti-Foaming Agent Fungicide Plaster 13A 0*10 0.750 170 0.25 1.875 U2 2.00 is.ooo 167 m. 0.50 1.50 3.750 11,250 9 3.25 24.375 11 5.00 37.500 196 .10 .750 126 .10 .750 - Sy./*-96v05 <$45<*?5 , 100.00 750.000 Adjust quantity according to set time requirements. - WORKING CONSISTENGY> Specifications - Refer to Plant Testing Procedure No. 32. Maximum Minimum Average 62. 58 60 SETTING TIME: Specifications Refer Co Plant Testing Procedure No* 6 (slow set) 90 rain. AO min. 60 min. WORKING PROPERTIES: Specifications Refer to Plant Testing Procedure No. 33. Must be plastic and butter/ working{ free of grit or coarse particles. BONDING PROPERTIESt Specifications Refer to Plant Testing Procedure No. 35. After compound has dried, tape shall delaminate when peeled back. .q^AC|LRES|sjAtSSi Specifications Refer to Plant Ted ting procedure No. 37. There ehall be no large fissure cracks In the wedge and very few, if any, cracks in the thinner half of the wedge. ^hnw`16j.oi.j2o EDOidok SGP 0018400 A -ia\. September 8, 1971 HEW FORMULA TEX-997 ACME. TEXAS PLANT FORMULA . SPEED SET JOINT COMPOUND WHITE TEX-997 (9 hour working aemant)^Houston Formula) DESCRIPTION OP PRODUCT? - Fox use in reinforcing and ooncoiling joints .and nailheads. - FORMULA Raw Material Function B.M. Spec. Percent Lbs/Batch Full Strength Commercial Retarder . Rotardor Hatrosol 230 UXR . , Thickner Celvatol RS-6278C Adhesive , Gelva GP702 Adhesive Asbestos SG210 Fiber Filler Asbestos 7RF09 Fiber Filler Mica pSOR . Antl-Craaking Agent Dafearner Mill Anti-Foaming Agent Panicide Fungicide Denscal Plaster i* 134 0.10 0.750 170 0.25 . 1.873 162 2.00 15.000 167 0.50 3.750 m 1*50 11.250 9 3.'23 24.373 11 * 5.00 37.500 196 10 .730 126 .10 .750 . - SY 7 86.05 . 645.373 100.00 750.00 Adjust quantity according to set time requirements, WORKING CONSISTENCYi Specificstions - Refer to Plant Testing Procedure Ho. 32. . Maximum . Minimum . Average 62 58 60 SETTING TIMBt Specifications WORKING PROPERTIESi Specifications Refer to Plant Testing Procedure Ho* 6 (slow set) 10 hours S hours 9 hours Refer to Plant Testing Procedure Ho* 33. * Must be plastic and butter? working; free of grit or coarse particles. BONDING PROPERTIES! Specifications Refer to Plant Testing Procedure Ho. 35. After compound has dried, tape shall delaminate whoa peeled back. - . CRACK RESISTANCE! Specifications Refer to Plant Testing*Procedure No. 37. There shall be no targe fissure cracks In the wedge and very few, if any, cracks in the thinner half of the wedge. . . NOTBt Set time measured by the first appearance of lumps in the mix,' EDO!dak Lehnert 10.3.01-121 SOP 0018415 fktv^X January 28, 1972 Supersedes TEX-997 Dated 9/8/71 ACHE, TEXAS PLANTLFOBWUfcA SPEED SET JOINT COMPOUND WHITE TEX-997 <9 hour working cement)(Uounton Formula) DESCRIPTION OF PRODUCT? - For use in reinforcing end conceiting Joints and nstlheeds. FORMULA -/ Raw Muturlal Function BsH*JLRS&* ,ta,rsmk I<k2/ich Full Strength Commercial Retarder Ratarder Natrosol 250 HXR Thicltner Gelvatoi RS-6278C . Adhesive Oelva GP702 Adhesive ' Asbestos SG210 Fiber Filler Aabestoa 7RF09 Mica p80H Defearner Mill Vaniaide Densest * Fiber Filler Anti-Cracking Agent Anti-Forming Agent Fungicide Plastor 134 0.10 O.'HS*- 170 0.25 1.875 162 1.50 11,250 167 0.50 3.750 - 4*73 13.123 9 . 5.00 37.500 11 3.00 37.500 196 .10 .750 126 .10 .750 m -64 3030 100.00 750.00 Adjust quantity according Co sot time requirements, WORKING CONSISTENCYt Specifications Refer to Plant Testing Procedure No. 32, Maximum Minimum Average SETTING TIKE: Specifications 62 38 60. Refer to Plant Testing Procedure No. 6 (slow set) 10 hours 8 hours 9 hours WORKING PROPERTIESt Specifications Refer to Flsnc Testing Procedure No. 33. Must be plastic and buttery working; free of grit or coarse particles. BOHOIUO PROPERTIES t Specifications Refer to Plant Testing Procedure Jfo. 33. After compound has dried, tape shall delaminate when peeled beck. * CRACK RESlSTAMQBt SpecIflostIons Refer to Plant Testing Procedure No* 37. There shall be no large fissure o?acks in the wedge and very few. If any, craqkp in the thinner half of the wedge, ' NOTE} Set time measured by the first appearance of lumps it) phe mix. EDOiets / denotes change Lehnert 10.3.01-122 SGP 0018416 A-\ I; '. . U4JL%/. czfc<) GLcwk --JL--i------- --- ;;. ; : -- - - chutld . _ .. *94 S&--Z./ 0 &&>l>>nu<g OtM^ / 2-J~7 2.5 y}fo*mpju*aiL /0-5-14-& aJh' 3/JT 4--2.T.-1^(Li/a^uc) SluiA^MJL J^L^OI QjfjEtA. MfriS-o1/- 77 S-3D-74 0S&IS /?7< 11-7-71 & Z-ZTS73 f_*.v /r i ^ 'v' y . - . l^fkei/ (Wal5t 1,9 * w 4-2ZP-7 2. fe f-/ 7-7 3 7*s4fetA 7-22-7/ -*1-77 2.* I1>7.2 },otr3.lS 6-ZSV 2/&A/ i ^.ehnert 10.3,01-123 [3 DEFENDANT'S 1 r ,, EXHIBIT 4Pa.- f &yQ chite, *}* St>-~LIu f'-tf-v to A*jf<Ufa 0Ut*> I - 20-7S ( uAr eb&c***Uuct^ I, 75 Q?kK-t s ^-17 C kjU- <yv6*&<\}Ms iAxud *c^ys/^sL &-- 2-1 O j^\jh l>0% 2. I cLa^s ^Hwz(x^/ (i/4 chte* ^aS^-'LtO C^utt^ C-2.1-13 to *t Uzsttr /,(. Qla+jt" f-v6>1? (^3*4/. ^t>cc4v^^r3 4*Jl3 i<r ,/rs- ....S6- >/6. No 042-1/0 '/o/01 /o / tehnert 10.3.01-124 i r O c^ytX &( yfjfi &**a fi&ei4m^J^ " scUotcj *ioS &--Z.I O ^/&u4/iAf Od/Zi!4***( 7'X7~72. G*iti Man e**d*fr/?72- &* ~ t*4**rt*M&*4 ^ 3d -7 2-j^er oUwf' t 5* iJW-StUu* , ^73. ^* Cwn/I&cn***! ^ 3" 30-72. a-^M^ / <5> Duxruc* V75 12. -Vl-Lf -tg. (g-4-77 A 25*4- 2,<9 (UJteujMi*1/70 &K**l 7-5 $ f 70 'j^Ji44H1A*e( &(7. J-<*-e{ 4LSMS &-2-fO ^faeJifi >*W tKT^TZcn A^-l ^Ae^fUc^S *faS6'~'Z(0 CUAffitfafecn. , 4eAi/^j // 5" * 3 -30~7X 4 <Lbw/'l/73 1,5 yizjtfiu&X Ci^h/S ^3 ~ 30 -~l cudi*/' ^/ry (,5 1TPtjfM $ j&&0 JSh* fe^t^yyiAf W-y-io^ 5-4-17 CfiulA CjA#Ufot7 /v*VMUA&u4 ctctA**^ sd/ziu Lehnert 10.3.01-125 I c^y{u**^ StC^-ltO , CzJafcj", f-i-=tf 4> / 2-/7^ Aje^jrUJt*/' I3-7-7 JT /[r ~* 7& J 'Cwrr'fcAj L&tsvyiuJ^kj 7" 2-7 ~77%, %~*-x-7 ^ &l<L '3-2-5'-7+ ----..^.^/lJi^4j(!ra )-* 44 in, 4 j jj u 3-^3^ <