Document mbqov4Odjy5M0LzDxQXqbJx2g

ir the purpose of research or private study only VALUATION OF THE CEMENT PROPERTIES ON THE PROMOTION OF ASBESTOS-CEMENT V. Ehrman Translation from Czech: Copyright Reserved There has been taking place for quite a long time discussions ween the manufacturers of asbestos-cement articles and oement as the characteristics of cement suitable for manufacture of asbestosent articles. On the one hand, one has to take into consideration production technology and the quality of the asbestos-cement lcles manufactured by using any speclfio oement, and on the other d the cement characteristics from the point of view of cement works ndards. Unfortunately it is not always true that cement satisfying the production standards is also suitable for the manufacture of estos-oement articles. The present artlole deals with a method table for the evaluation of the suitability of oement for the ufacture of asbestos-cement articles. In the course of time there have been specified various requireta for the quality of cement suitable for the manufacture of estos-oement artioles, for instance the degree of grinding, speoific face area, compression strength, start and finish of setting, aioal and mlneralogloal composition, but all these requirements were aulated mainly on the basis of prolonged empirioal experience, thermore, up till now, it is still not quite olear why cements of liar or even the same chemical or mineralogioal composition behave te differently under the conditions of manufacture of asbestosent articles. Cement constitutes 85-88^ of the asbestos-cement mixture. Thus is extremely desirable to have a method for the evaluation of the ent characteristics prior to its use in the manufacture of asbestosent articles. The existing methods for the evaluation of oement a a /2 C7D028902 2* ility are baaed oa lta use as a binder for eoneretee and mortars, 1 la Oseohoslovakia this characterisation le oarried out according standard G3H 72 2121. In the ease of the manufacture of asbestosisnt artlolse the process oondltlons are quite different, and thus roes should be placed on different characteristics of cement. Abroad, use Is being made since the fifties of a method reloped at Johna-ISanville laboratories specifically for the iluatlon of the eharaoterlsties of oement, whloh is to be used for e manufacture of asbestos-oemest articles (1). This method is lied the Sag-Test and is also known in Europe (2). This method kes it possible to determine the plasticity of the fresh aabestosaent material, the amount of water retained in the articles after 8 shaping and pressure treatment, density of the set article and 8 bending compression strength. Slnoe these studies are oarried t by using the same raw materials and the same production oondltlons d only the ca*ent/iie4ting ohanged, then the changes in mixture araoteristlea may be assigned to be due to the cement. This thod is baaed on the determination of the degree of plastlolty of r asbestos-cement mixture by establishing its deflection from the risontal under the motion of oonstant load* O-TEST METHOD. The equipment used for this test is illustrated schematically t Fig.1. In this test there are used 32g. of asbestos fibres, g* of siliceous flour end 80g. of the cement being evaluated* tie mixture is first dry-blended for 10 minutes in a drum rotated ; 90 rpm, and in the aotual test 150g. of the resulting mixture 'S used. The weighed sample is mixed with 1000 ml of water ?1C, pB 6-7) for 1 min. at 900 rpo. The time indicated in the .notable presented in Pig.2 is measured from the Instant the cement )mes Into contact with water. The resulting slurry is transferred mediately to a filtration vessel and in 1x19 min. the water limination is commenced. A vacuum of 409 ton? la maintained, s the course of the dewatering and formation of the asbestos-cement ke one must ensure that the ooapaction and evening-out process ake pises under strictly defined conditions, and the pressure is ...*/3 CTD028903 o maintained at a strictly defined level. The Bebeetoe-oement a la maintained under vacuum for 3 min.45 see* and then is taken of the dewatering vessel. The saae conditions are need for the paration of four asbestos-oeaent oakes. The shaped oaks is weighed in the coarse of the next 30 seo. and a Its density after ooapletlon of the filtration process is abllshed. The weighed oaks is then subjected to a pressure of 4 kp/om2 (320). The pressure treatment should be started in 50 ain.f a maximam pressure should be attained in 7 * 00 min** and pressure should be maintained for 7t05 min. Then the pressure reduced and the pressure formed plate is removed from the press* The resulting plate is weighed and then is placed in the instruaen d for the evaluation of its bending strength. The micrometrio loator should be eet to sero* After placing of the plate in ition the indicator indicates its thickness, and at the saae time position of the handle lndicatea the initial value for the Sag-Teat ruination. In the course of 9*00 min., the arrester of the troment le released and after 10.00 min. the deflection value is irded. A total load of 140.0g. ie applied to the oentre of the te, and the distance between the plate supports is 152.4mm (6 fingeri value of deflection Is measured accurate to three places of deoimali llfferent for different cements and in general lies in the range ,060aa. After the measurements have been completed the cake is again med to settle, and then is placed for 24 hours in a thermostat at 5 and min. 900 relative humidity. Then the plate is transferred in autoclave and la subjected to a pressure of 7 kp/oa2 (saturated in temperature of about 170C) for 16 hours. Finally the plat# maersed for 24 hours in water at 23C* After this treatment the mass of the saturated plates in air and ir is determined. Then the breaking test is oarrled out and tore tbloknene le measured. The sample is then dried (100-105C, ours) and after cooling ie weighed. *../4 CTD028904 4 The measurements, whioh have been taken may be need for the ilculatlon of the following parameters! the water oontent of the ?esh sample after filtration and after pressure forming* the )nding strength of the plates and the absorption and density of xe plates formed by using the oement under investigation. The imblnation of the plastlolty of the material and the value of its mdlng deflection constitute complex parameter of the oement being ied. mCHJSION It may be ooncluded on the basis of the studies carried out ' Johns-Manville on various types of oement and in the oourse of ie last fifteen years that the behaviour of oement under the mdltlons of manufacture of asbestos-cement articles is quite .fferent from its behaviour in the oourse of concrete production, ie Sag-Test is capable for elucidation of some fundamental taracteristics and is suitable for use in the asbestos-cement ehnology: The temperature of the charge water has a positive effeot on ment plasticity, i.e. the higher the water temperature (in the nge 16-30C), the higher will be the plasticity (higher deflection). The plastlolty of the plate is Inversely proportional to the ter oontent, i.e. the greater the deflection the lower will be e water retention. Thus for instanoe cement having deflection 2.540mm has water retention of 27-28$, while cement having low flection, e.g. 0.508mm, has water retention of 32-33$* The low water oontent of the plate results in low porosity ter curing, and thus low water retention results in high strength, r instanoe, oement having water retentionOof about 28$ can be used prepare plates of strength 295-309 kp/om , while oement having ter retention of about 32$ gives plates having a strength of only 6-253 kp/om^. The introduction of the Sag-Test method in Czechoslovakia would rtainly olarify the problem of suitability of various cements for 9 manufacture of asbestos-cement articles. bliography. Johns-Manvilie Corp., Manual of Test Methods, Method No.425*11, Aphflfrfc--nn.-V.1or> -w -- v 1- .ewr*. CTD028905 re Captions 5. 1i Schematic representation of the 8ag-Test equipment* blending fonnel; 2 - trough; 3 - filtration box; 4 - anotion k (2000 nl); 5 - meroury manometer (500 torr); 6 - air aspirator; device for manual tamping of the oake; 6 - smoothing spatula; support for the oake; 10 - plate for transfer of the cake; weighing balance (250g accuracy O.lg); 12 - laboratory press aslng force of 5500 kp); 13 - Sag-ffester; a - air inlet; projection; A - filter paper; B - test oake; C - sieve (20 mesh) two sheets of filter paper; - perforated plate (6.4mm openings); four sheets of filter paper; G - perforated plate (12.7mm open- ). Pig.2..../6 CTD028906 6. 2,. Tine eohedale for Sag-Test v___________ weighing after filtration_______ ---------------------------------------------------\ t---------------. pre88ur<} treatmeiit V. ' weighing after pressure treatment ________________ deflection determination wet settling 32C, 90 rel. humility \/______________________________ autoolave treatment 7kp/om2" ,>"s--a---t-o--r-a--t-e---d----s--t-e-a--m-- 16 hours 1 water storage 1 24 hours 1 final testing. 1 6.30 min. 7.05 min* 9*00 min. 10.00 min. end of test 24 hour8 CTD028907