Document kmyg99k3DpdeBGLBnmgYNzj9V

DURABILITY STUDIES OF REX 45QOO - KM BULLETIN YiHITE rtion and iscope: This report describes the res\ilts obtained from a series of expo- % experimental formulas of Rex 45000 - Kem Bulletin White. The variations changes in pigmentation and in vehicle composition. Tte believe that the phase, that of studies of vehicle changes, give worth while Information as comparative durability charactei'istics of linseed-perilla combinations, i l, and soybean oil types of synthetic vehicles. ition and Methods of Exposure; The exposures were ell prepared on o" x 24" galvanised iron panels, at coat was Galvite Primer - Rex 26440, reduced 25? with mineral spirits Hod 4 hours (in the laboratory). The second coat was the experimental 3, reduced 12-1/2? with mineral spirits, and applied to the upper half of si only. After an additional 24 hours of drying, an ovor-ull coat of the ital Rex 45000 was applied. Thus we have in effect both the conventional st and threc-coat systems, ac'mouledging that a difference of drying appears (application of the final cost (46 heurs on the primer between coats for it system vs 24 hours between coats for three-coat system). On each panel the "A" section is the three-coat area, and the "B" the two-coat area. The panels were placed on exposure, 4.5 south, on our Chicago expo^arm, on 8-20-56, and the exposures discontinued on 5-20-37, representing & nine months' exposure, largely during winter months. 0007-SWP-045350 0007-SWP-000114721 itary Report 'Weeks' Panel Exposure The condition of the panels carrying the synthetic enamels and s, made with the variously treated titanium dioxides, after six and twelve ' exposure respecttveJ.y at 4C facing south in Miami, Florida, is tabulated White PlpTr.ent Titanox-A LO Krebs LO Zopaque LO Titanox-A LO 'Krebs LO : NC Titanox Krebs LO .Titanox-A LO Krebs LO :Titanox-A LO Antimony Oxide Krebs LO Antimony Oxido Krebs LO Antimony Oxido Titanox-A LO Antimony Oxido Treatment- of Titanium bioxide Pulped Ground tJaleutcu Pulped Pht-haiatod Pulped Fhtha.lc.ted Pulped Pulped Mr.leated Pulped Phuhalated Pulped Chtdking ..6. v^eks None Chalking 12 'Peeks Very slight Moderate Very slight Slight II None Very slight None Incipient Very slight Slight Barely perceptible Incipic-at 0007-SWP-045351 0007-SWP-000114722 ki i LO ^Antimony Oxide I'Titenox-A LO KZinc Ti tana Co |. Krebs LO I zinc Titanate ^Krebs LO i'Zinc Titanate |Titenox-A LO |zinc Titanate prebs LO KZinc Titanate |Titanox-A LC fcbad Titanate K',- x prebs LO picad Titanate Prebs LO gad Titanate pitanox-A LO Kecid Titanate Krebs LO [goad Titanate 18 Phthalated Pulped Pulped II Chalking 6 Weeks None Incipient ff Chalking Very slight Moderate, bad fading ii it m Staler, ted Pulped Phthalated Pulped Phtbnl r ted Pulped Pulped Pulped Hone II II 11 Incipient Incipient II * U Moderate, bad Ending tt It II Ualur.tcd Pulped Phthclatod Pulped Phtvjatcd Fulped None n n Barely perceptible II M Palced flight Bad 0007-SWP-045352 0007-SWP-000114723 Treatment of Itanium Djoxide- Ground Titeno>r-A MO Antimony Oxide Krebs FF Antimony Oxide Zopaquo Standard Antimony Oxide- Krebs Antimony Oxide Male-nit d Pulped Philinlatod Pulped Pulped Maleatod Pulped Chalking S books Incipient IT Slight Mone Flight It None Slight II Moderate Slight II II hone ii Incipient II hone n Chalking 12 Weeks Bad Moderate Bad Moderate Sovorc Bad Incipient Severe M 1! Moderate Bad 11 Moderate {fading-) Moderate Bad n Very slight ti ii 0007-SWP-045353 0007-SWP-000114724 Treatment of Titanium Dioxide |S FF jtinony Oxide Phthalatcd Pulped [tanox-A MO [j bc Titanate ` bs FF Sc XitanatG *f?> f Spaque Standard Sc Titanate Pulped II M bs FF C TITANATE Kaleatod Pulped FF "Titanate Fhthalatod Pulped x-A MO ad Titanate eb3 FI' _ Titanate Standard ^Titanate *F? Ltonato FF ijTitanatc Maleated Pulped Phthaln.ted Pulped Chaining S hooks More Incipient Very slight Mono Slight Incipient None C halking 12 Weeks Moderate Bad 11 Moderate Incipient !! Severe Moderate Severe Slight .t Practiced in tlr.s investigation is ineffective in deferring the the TiCa or in lessening its severity. or tnalection, i.e. surface coating the pigment with titanium Stc;*l titanium maleate respectively, is quite effective in deferring the 0007-SWP-045354 0007-SWP-000114725 -a- tg of TiOg lessening its severity both in synthetic enamels and ucr. ference in chalking tendency of the TiOg pigmcait, from different sources crent. In order of chalking they are as follovrs: Zopaque, least; jx-A, intermediate; Krebs; most. The difference is too slight to offer rcat margin of safety, The Burgess Experimental TiOg is quite resistant Iking, but lacks other desirable pigment properties, line titonatc end lead titnnato behave in r. most unsatisfactory manner in or.. They apparently induce excessive fading and in 33-1/3? admixture vJith gted TiOg do not affect chairing rate. In this same per cent admixture htholuted or maloatod TiOg behavior is more normal, titanatc, zinc titanatc and antimony oxide in 33-1/3? admixture with TiOg offer little or no, protection in deferring or lessoning chalking. In order to determine the effect of the phthalatod pigments and sad titunate on drying time of the synthetic enamels, the following 'e chosen: Synthetic enamels made for this work on March 18, 1937, and which Ta storage for five- months. The chito pigments in the enamels arc as (vl.- Untreated iitnnium Dioxide '2. 5? Phthalated Titanium Dioxide ^3. 5? Maloatcd Titanium Dioxide ,4. Special t<on-chalking Titanox-A |j* 33-1/3% Load Titannte, 66-2/3? Titanium Dioxide tif' 33-1/2^ Zinc Titanatc, 66-2/3? Titanium Dioxide 0007-SWP-045355 0007-SWP-000114726 These cnsuseIs were sprayed one coat on steel panels and compared -cshly prepared cnaacl, made on the sane forcula and in trhich the v;hite 3 untreated titanium dioxide, for drying; time. Wo difference was .apparent in the drying rate of the sovon enamels. In order to test fully the value of phthalation of titanium dioxide, 'wing pigments vvill be prepared, made into enamels and lacquers on the 'giver, in the first report on this subject, spreyed on panels and exposed 1. Control, untreated Titanox-A 2. Titanox-A - phthalation 5. Titanox-A - 5% phthalation 4. Titanox-A - j.CP phthalation 5. Titanox-A - 15^ phthalation 6. Titanox-A - treated only vrith phthalic anhydride There v.iil be included with those exposures panels prepared using ?hollcing Titanox-A, prepared by The Titanium Pigment Company, tho method t of which bus not boon disclosed. - Further reports will follow. 0007-SWP-045356 0007-SWP-000114727 fc L/a\) Colloid Chemistry" - Vii 1 etci' 1. b^ncroft. Chapter I. Adsorption of jfepor by Solid. iicGrav,- Hill BooY. Co., 2d Edition, Pace- 3. Filuc" - Chapter 2. Principles of Cheated Engineering. Walker, McAdams. HeGrav; Kill Bo o k Co ., 2d Edition, Page 56. [ition cf Solid by Liquid" - Wilder D. Bancroft. Applied Colloid f, 2d Edition. MeGra.? Kill Kook Co., Page 100. tes" - H. A. Gardner. Industrial and ihginooring Chen., Vol. 28, pfitanate" - D. VI. Robertson. Industrial and Engineering Chew. |g8, 1956. Page 216. 000 7-SWP-045357 0007-SWP-000114728 0007-SWP-000114729 After-Bodying of Lithopone paints is closely related, to the surface JS'*. fiof the Lithopone particle and presents a type of phenomena somewhat ^rom that usually associated with normal consistency values. Today under the concepts built up by physicists this latter type Svity is now considered to be both physical and chemical. The forces otrol surface reactivity operate in addition to those of a more purely ^character, usually associated with wetting phenomena and upon which Lithojfistency evaluations have been generally based. The study of surface phenomena is in its infancy, hut sufficient re known to servo aB guides in determining the suitability of Lithopones purposes. Wettability and consistency phenomena are discussed in Reailetins 11 and 12 - "Wetting and Dispersing Agents in Paint Formulation," 8fe" rotednre for Evaluating Lithopone as Regards Consistency." Several designations have been used to describe surface reactivity ,to Lithopone, among which "surface attraction,11 "adsorption capacity." gjjic&l chemical attraction" have been selected as most self-explanatory, of simplicity this type of reactivity will be expressed by numerical Seated as the "P-C" factor (p-C = physico-chemical). This reactivity to be related to a physical condition of the surface of the Lithopone feather than to a distinctly chemical condition. This physical condition W,. related to the character of the porosity of the surface and those forjv . ^_pperate in and on micro-cellular structures as well as to the atomic the surface molecules. 0007-SWP-045359 0007-SWP-000114730 - p. - 9f! ffif- conditions which favor the production of a finely particled LithoMr Ifreased surface area3 - with increased surface porosity of which the high KV Lithopones are typical, produce Lithopones of high surface reactivity, fitting characteristics. Hence over-calcined Lithopones of larger par- ore generally of low surface reactivity and good wetting qualities, jawing table shows typical P--C" or surface reactivity factors for several Xf Lithopone as determined by the standard procedure given under a subse- Tabls I "P-C11 factors According to LlthOponc Grades Lithopones ,rP-C" factor Low consistency L, LL and low li ranges Medium . " High M, H and S ranges High 11 H ranges 3-5 to 5-0 5-0 to 6.0 6.0 to 9-5 In the middle consistency ranges a "P-C11 factor in excess of 6.5 pected to show after-bodying characteristics with sensitive vehicles, hofee which contain polymers not far removed from the gelation point. Soap treated lithopones - those which have received a treatment Hj^.Qcid. soap3 of complete or partial neutrality, usually have a surface approaching zero, since the attraction has been neutralized by the Sj-agent. Therefore, it is possible to reduce the surface reactivity of a jgthoponu to any desired point by the addition of definite amounts of such 0. the Lithopone "in the wet." It has been observed that Lithopones of high pH value can show a Efface reactivity or "P-C" value than would bo expected from their k^ty nnd the reverse condition has also been noted. 0007-SWP-045360 0007-SWP-000114731 to Surface Reactivity v jpjje general precise, that maximum Lithopone production and ccnsumpt'i - ?ibo directed to three types of Lithopone - a low, medium, and high con-, ^should he kept continually in mind by the technical men associated with Sjjroductian and ty the paint formulators and superintendents, if special ^grades are to he reduced to the minimum. To meet this plan adequately, these three grades of Lithopone must ^general purpose" type, which will not react to an appreciable extent jitive" vehicles, possess excellent mixing and grinding characteristics int consistencies in line with the established "A" and "B" consistency :, above all, a ''general purpose" Lithopone must be relatively face reactivity or "P-C" factor. The high consistency Lithopones constitute a partial exception', as gable degree of reactivity is associated with increased consistency, elf limits their general usage, and makes it necessary that with such the nP-C" factor be closely controlled. Poor wetting Lithopones, i.e., those having a high adsorption |moy behave normally as to their consistency characteristics in those possess a safe solvency balance between the various polar constitand also between the non-polar and polar constituents. {Mineral non-polar, fatty acids the most active polar, and oils according polymerization of varying polarities). Such poor wetting Lithopones may exhibit normal "A" and "3" con tactor^ tut if used with a "sensitive" or tinbalanced vehicle, i.e., one fi- threshold of gelation, may show an abnormal increase in consistency, 0007-SWP-045361 0007-SWP-000114732 r exhibit marked after-bodying characteristics, resulting in cusjf ' ixsts unless caught by the paint factory personnel. k. ggy rfjj.e use of these "sensitive" or unbalanced vehicles in paint factory os non became so widespread, that aa appreciable degree of reactivity ^rmltted in deliveries of "general purpose" lithopones, if paint factory jur complaints are to be avoided. Vehicles may be "sensitive" to surface reactive lithopones as to neither initially, or on storage, for a number of reasons, most of which to phases of polymerization and solvency. A reactive Lithopone may ^remove from solution in the vehicle, a sufficient quantity of the most constituents - fatty acids of varying degrees of polymerization - and s primary and secondary envelopes on and adjacent to the pigment par- 3, to reduce the solvency of the high polymers in the balance of the ~the "gelation point" causing the paint to thicken. This preferential adsorption and orientation of these polar bodies the pigment particles is a time reaction and hence may become after-bodying. Again, a high concentration of a non-polar constituent in a vehicle E?.Ye type, as is frequently the case in traffic zone and flat wall paints fi uxo produce after-bodying with reactive lithopones for similar reasons. The formation of enormously high polymers of low solubility, such ryn `Lc'-rge quantities in the highly heat-bodied oils (10 minute to 20 minute "IT tube) are not only a source of high initial consistencies with surface opone pigments but are also a frequent cause of after-bodying. 0007-SWP-045362 0007-SWP-000114733 -5 - China Wood Oil Varnishes in which the oil has been highly polymer'enolic Resin Varnishes in which the resin has not been completely "'frequently show after-bodying troubles with surface reaction Lithopon.es. cations of the Above Principles The following illustrations indicate how the reactivity or "P-C" a Lithopone influences the consistency of paint factory productionswhen the types discussed in the above caption are used. Two production lots of Lithopone of similar wettability character.^Shown by the fallowing "A" and "3" factors but with widely differing 6rs were tried in a typical traffic zone paint. Table II Lithopone Characteristics ? - "A" Pact or "B" Factor wp-C" FactorInitial______After-BodyInitialAfter-Body 11.7 5-7 19-2 18.9 + 7-2 sec. + 0.3 " 21.8 20.2 - 0.4 sec. + 0.4 11 5f-: The Lithopone with the high reactivity of 11-7 gave excessive i&g of the traffic paint iD question, while the other Lithopone having .actor of 5-7 showed normal initial body and the paint maintained that |0_n storage in the can. The effect of a highly surface reactive Lithopone compared with lithopone converted to very low reactivity and both used in the manu- flat wall paint is shown in the following table. This Lithopone was ^ M consistency range and the "P-C" factor normally should have been-be 5. ana. 5.0. 0007-SWP-045363 0007-SWP-000114734 i rr Table III Iiithcroone Hat frail Paint Consistencies* 1 Day 2 Dsys 4 Days 7 Bays 30 Pays 1970 sec. i)490 sec. 23 11 25 " Too thick 30 sec. Too thick 34 sec. Too thick 32 sec. i'er viscosimeter, seconds for 50 revolutions with 35^ grams. In obtaining high initial consistencies of products such as painter ft?.;. tithe so-called "ono-coat" type, use may be made of Lithopones of a high ^>r. If used with a poor netting vehicle containing a large percentage olymers, this abnormal consistency can be maintained on storage in the isiderable periods of time, thus overcoming one of the difficulties Rencountered in this type of enamel production, viz., the "sliding off" usistency within a few weeks of the date of manufacture; _A Lithopone having an "A" factor of 26-H seconds, a "3(l factor of ja-nP-Cu factor of 9.1, mixed and ground in a highly polymerized Sardine fervehicle, and thinned with a China wood oil-Perilia-Ester vehicle in gChina wood oil ha3 been brought close to the threshold of gelation, rename 1 of abnormally full consistency, which held in the can. If the ^allowed to stand over night a further marked increase in consistency |tlf the grinding temperature was raised from 125 F. to 154 F. the Wed an increase in body from 475 seconds (stormer) to 1070 seconds. Other similar experiments showed that grinding temperature played an goie.' It is believed that with a vehicle of the above characteristics, ||ftive polar constituents are able to attach their molecules so firmly gncs of the Lithopone particle that they arc not dislodged on storage 0007-SWP-045364 0007-SWP-000114735 can. They thus maintain intact both the primary and secondary envelopes j!the particle which in uur,, doto.'r.tr;.'. structure of the mss and the -jty of the enamel. Inci-cu.m-. 1 . - ..ili. in the setting up of the t rucluxe. nation of tile "P-C11 or Surface Hoaetiv.ty factor Tlie following procedure developed by Ct 3)* Dofens is considered an ite measure of the surface r ..activity V.tliopone pigments. prun.i of pur. .inneed fatty acids required to effect iis-or of '.iC-'; grams of a pigment suspended in a non-pilar1 .or,nil (mi'em.. spirits or naphtha) is taken an th? Ai.i..yption factor, or "P-Ca factor Cf that pigT.-,.i . obtain*.! ly : linseed oi act./ is eefined as the product filiation of a sulphuric acid treated airing cr act. 1 value of 200. Ifote: Linseed oil fatty acid (212'j) c.s obtained from Wecoline Process Company or 7obam degreasing Company is speci fied. as: Acid value, 195 minimum.; iodine number, 195 minimum. At 195 acid value it would therefore, for purposes of this tost, bo considered as 97~l/2$ pure. The V212C) should be fresh and very pale in color and produce a solution clear and colorless. It should be stored in full, amlor glass- containers. .Standard Linseed jr.V:t,y Arles Scl:y. u (a) Dot emino vc.ey aoourctciy and cxa.cc ly the acid number of the (2120, used. Tnii. a: done frequently to chad-, on any deteric ?ot \r ito', may occur. Be sure aaiaplo is re present a ,:.-v -. (b) ''oigh accurai-oly into 5'uO i-c. volumetric flask (2120) equal to: 10 ,crane z 200 Acid So. of (2120) Uss capr-oJ. neighing pipette. Avoid losses during transferring. loop (211C, homogeneous while weighing, m to oi 0<10 1 SC tIo f' o o o 0007-SWP-000114736 Make up with clean, water-free (3^8) to exactly 500 cc. Assuming the acid renter cf Pare Linseed Patty Acids to be ?0C, tk'.c cc hit ion contains exactly 0.C2 grams/cc. of Tv.:Linseed Fatty Acid. If the weight of the fatty acids is not exact, this is taken into ecrk ..usration by calculation in establishing the value of the solution. For example, assume the ac.id value to be 19S. The amount of fatty acids for 500 cc. of solution would be: 10 grams x 200 ,, 10.101 grams 19S If the weight actually added however was 10.200 grams, the value of the solution, cast be cal culated by determining fatty acid, per cc. (di viding by pCO) to give 0,020h grams and multi plying by the factor representing the relation ship cf the acid value to "CO. In this case 198 x .0204 to give the value of 1 cc.of the 200 solution as'0.-0202 grans pare linseed fatty acids. 10 grans of pigment is accurately weighed and transferred to a glass slab. Five ec. of (348) - mineral spirits is then added to the pigment end worked in with a spatula. The linseed fatty acid solution is then added drop by drop from a burette, working in well and mixing all thoroughly with the spatula after each addition. After the addition of the first few drops a heavy, short or flocculent and thixotropic paste will result. As continued additions of the fatty acid are made the paste gradually loses its flocculent character and the end point, disappearance of thixotropy, is 6harp. cc. linseed fatty acid solution taken, multiplied by 100, multiplied by the value cf 1 cc. in terms of pure linseed fatty acids is the Adsorption Capacity Factor of the pigment used. . _of Linseed Fatty Acid Solution The solution deteriorates and breaks out on aging, consequently Uacd when fresh and not used when more than a day old. Great care ^ in holding this solution at standard value. 0007-SWP-045366 0007-SWP-000114737 We. 9f 9- Cfiaa Element In order to stabilize the tine c.l.cnont...ond allow sufficient tine Kfor making the mix thoroughly hoaegeteou-: after each addition of the fatty Ifsolution, each tost should consume 25 - Z'-` minutes normally for lithopone Ks lesi jfedeoiPt The endpoint, defined, as disappearance of all flocculation, is by gathering up all the thoroughly mixed paste into one pile when the at is approached, end drawing the spatula lightly over it to spread it out lick layer on the slab. The nix, at the endpoint, should spread absolutely tidy with, no tendency toward unevenness, It juicing, or flocculation. The should not pile up "slushily11 in front of the spatula as it is drawn over Should flow smoothly under the spatula. If po.rticles of the nix become dry fv'is spread out thinly, and are gathered into the rest of the nix, they should ||e confused with the flocculent nature of the wet paste before the endpoint is ft fed. llornal pressure is used on the spatula while nixing in order to i up pigment agglomerates and allow thorough and smooth incorporation. (ft Ijhifornity of Deliveries 3ascd on "P-C" Factors It has been pointed out that the "F-C" factor can be controlled by jtially neutralizing the surface attraction of the Lithopone particle to any point by neons of treating agents during manufacture. Hence it is possible Reduce successive batches of Lithopone having the "P-C" factor held within -.B runges. a high consistency Lithopone, therefore, nay or nay not have a !j-. ,f~C" factor. 0007-SWP-045367 0007-SWP-000114738 9f - 10 - Eight successive deliveries of a competitive Lithoponc having an or of 32-H seconds and a "B" factor of 37 gave "P-C" factors within the 4.6 to 5-6-' Sight hatches of Coffoyviile production with on "A* factor 15-H to 19-H seconds gave "P-C" factors of 7-9 to g-9-. Seventy-six in the middle consistency range of 15 to 26 "A" factor cane within a of 5-0 to 6.1. The margin cf safety necessary to prevent aftcr-bodying is daon the sensitivity of the vehicle used and. the paint fomulator must to Ihy his own findings. It is desirable that tho different lahorctcries familiarize thenJwith the details of the test and know that they can check their findings ose of other laboratories through the use of a standard Lithoponc having "P-C11 factor. I lli 0007-SWP-045368 0007-SWP-000114739