Document km5r1jbbn89LrGRrVmVLb16b

Return to: CDRDept Jackson Latioratory R. 4 D. File Room ii Return to: CDPDept Jackson Laboratory R. & D. File Room l! Return to: CDPDept. Jackson Laboratory R. & D. File Room r Return to: CDPDept Jackson Laboratory R. & D. File Room Return to: MU-1M0 <Rv. 3/711 CDPDept Jackson Laboratory R. & D. File Room E. I. DU PONT DE NEMOURS & COMPANY 256 VANOERPOOL STREET * NEWARK, NEW JERSEY Serial No. KN-69-2 Copy No. // NEWARK PLANT PIGMENT COLOR RESEARCH REPORT BT-449-D - QUALITY IMPROVEMENT Pariod Covorod March, 1967 -- January, 1968 FILE: 223.41 DATE: 1/2^69 NJ 9346 DUP050081276 KN-69-2 X. Numerical File 2. Research Office File, Newark 223.41 3. Newark Library File 223.41 4. M. Hunt/E. Gonick, Pigts., Wilmington 5. W.s.Struve/A.A.Brizzolara 6. F.F. Ehrich/B. H. Perkins/H.H Syorgy/Library ?. P.J.Monahan, Newark (Vital Records) 8. N.G.Fisher, central Research, Wilmington 9. R.H.T'etzel/J.F.Maurer/J.W.Minnich, Newport 10. E.E.Jaffe 11. Extra 12. Extra 13. Extra 14. Extra 15. Extra NEWARK PLANT PIGMENT COLOR RESEARCH REPORT SUBJECTS BT-449-D - QUALITY IMPROVEMENT Period Covered? March, 1967 - January, 1968 SUBMITTED BY? E. E. JAFFJ APPROVED BY: A. A. BRIZZOLARA Date Submitted 12/1/68 Date Released; 1/27/69 DUP050081277 TABLE OF CONTENTS I. HISTORICAL INTRODUCTION II. CONCLUSIONS III. ACKNOWLEDGEMENT IV. DISCUSSION 1. Mechanism of Breaching 2. Desirable Properties of Breaching Solvents 3. Emulsion Stability Considerations 4* Breaching with ccl4 5. Dispersibility of Plant CC14-Breached Products 6. Migration in vinyl and Hydrolysis of CC14 7. Perclene as Breaching Solvent 8. Perclene - Emcol P-10-59 Combination 9. Plant Breaching with Perclene 1 1 2 2 11 13 14 cm u> vo oo oo c* DUP050081278 I. HISTORICAL INTRODUCTION BT-449-D, a breached semichloro copper phthalocyanine (CPC) specifically designed for easy dispersibility in vinyl was intro* duced to the trade by DuPont in 1962, The pigment found fairly wide acceptance for pigmentation of plastics and some application in inks. The preparation of this pigment entailed breaching of pre milled CPC containing 3,8 to 4.5% chlorine with ortho-dichloro benzene (ODCB) followed by batch distillation of the organic sol vent, acid extraction, pressing, laking with 5% calcium Staybelite, drying and pulverization. All processing steps up to the laking procedure were carried out at Newport and the remaining steps at Newark Unfortunately, since the introduction of this code, there has been a nearly continuous quality problem of borderline or inferior vinyl dispersibility as determined by minimus* dispersive effort, such as five cuts in vinyl on a two roller mill, strength by rdbout has similarly been variable and frequently outside Shipping limits. Several processing difficulties were recognized by J. H. Braun and subsequently P. L. Re&g. (1) The chlorine content in the pre-milled crude was frequently outside the designated limits. (2) After apparently complete distillation of the breaching sol vent, the product contained substantial amounts of ODCB. To eliminate the latter difficulty, studies were initiated to (a) use a flash distillation unit for complete solvent removal and shorter and more controlled contact time between the ODCB and pigment, and (b) use other less potent and lower boiling solvents in the breaching operation. A study by D. H. Eastham* led to the installation of a flash distillation unit at Newport, The demonstration that carbon tetra chloride (ccl*) can serve as a breaching solvent (patent proposal J.H.Braun #1603-K) led F.L.Reig to work out a process using a specific surfactant (G-3300) which gave good results in laboratory experiments. Although the introduction of the CCI4 process in conjunction with the flash distillation unit into the plant had a beneficial effect on pigment dispersibility, in general, plantproduced pigment continued to be dull and reproducibility in dis persibility was not good. In addition, a serious corrosion problem was encountered in the Newport plant. II. CONCLUSIONS It has been demonstrated in the laboratory, Semi-Works, and the plant that BT-449-D of good quality, requiring no extenders, can be produced by extensive modifications of the old process. The changes involve the substitution of perchloroethylene (Perclene) for ODCB as the growth solvent, improved emulsification of the Organic solvent in the pigment slurry, change from batch to flash distillation for removal of the organic solvent, and an improved extraction procedure for the removal of base-soluble im purities and a substantial part of the emulsifying agent used to promote emulsification. *Report KN-67-15 DUP050081279 -2- A problem related to the tendency of the pigment to bleed under certain filtration conditions from alkaline medium remains to he resolved at Newport. Progress has been made toward the resolu tion of this problem* XXX. ACKNOWLEDGEMENT Close and effective cooperation during the plant phases of this investigation from F.L.Reig (Newport)and R.F.White (Newark) is gratefully acknowledged. XV* DISCUSSION The approach to the solution of the problem has been to determine the basic parameters in the breaching operation and sub sequent processing steps which are responsible for variations in dispersibility and strength of b t -449-d . 1. Mechanism of Breaching One of the first requirements in this study was to find a physical method for rapid and reasonably accurate determination of the primary particle size in a breached pigment, either directly or by a proportional parameter. In addition, an accurate deter mination of the amount of 0-CPC present in a breached product was desirable. To determine the amount of 0-CPC in a breached product with some degree of accuracy, a series of mixtures of a-free 0-CPC (BT-297-D, lot 00994) and 0-free a-CPC (BT-304-D, lot 00704) were prepared (1869/3). The mixtures contained 2.5, 5, 7.5, 10, 15, and 20% 0-CPC. A plot of the 9.2 to 6.6 20 peak height ratio vs. % 0 phase content as determined from patterns obtained at l/min, was linear at low % 0 content but curved off at higher percentages of 0 phase. A straight line was obtained over the entire range of concentrations when the peak height ratio was plotted against the ratio of % 0 over % a-CPC. A similar plot was obtained from patterns run at the regular speed of 2/min. This method is reliable provided the measured a- and 0-phases possess the habit exhibited by the standards used in the prepara tion of the reference plot. Xn an attempt to determine primary particle size, the easily measured 0x/a (half width of a prominent peak in the X-ray diffraction pattern) could not be applied in this case since the prominent peak in the X-ray pattern is a doublet and, in addition, most products contain variable amounts of 0-CPC making the determination of 0x/2 on most peaks an unreliable measurement of the particle size. Fortunately, the use of the so-called valley parameter* due to the valley between the peaks at 26.6 and 27.5 20 values is not interfered with by the presence of small and variable amounts of 0-CPC. The valley parameter (v.p.) can be defined by the expression AB x 100 based on the drawing in Fig. 1, where AC 2 *C.W.Manger, Report KN-68-4, p.10 N DUP050081280 *3 - It is simply the ratio of the distance from the lowest point of the valley B to the point A located at the average height of the two neighboring peaks from a common baseline, and the average height AC. When the ratio is multiplied by 100, the v.p. values of all products prepared in the present study fall between 30 and 80. The larger the v.p., the larger the primary pigment particle size. The validity of this assertion is based on comparisons of physical data obtained on pigments breached with various organic solvents. . By measuring the v.p.'s on a series of carefully breached samples prepared by P. L. Reig with variations in the amount of o d c b used as well as the duration and temperature of breaching, it became obvious that particle size growth occurs during the breaching operation. The data compiled in Table I show that when using the same premilled crude, which is itself very poorly crys talline, a series of breached products are obtained which show an increase in v.p. and % 0-phase content when either the amount of organic solvent, the temperature or duration of breaching is in creased. Moreover, all other things being equal, the larger the grown particles, the more dispersible the final product* Temp. Duration QDCB/ of" of CPC Breach., Breach. ,163 25*0. 22 min. .163 25 120 .163 95 127 .489 25 120 .489 95 15 .630 28 128 .630 90-98 15 .630 90-98 127 TABLE I Strength vs.BT-449-D.TS97419 Surf, V.P. Area % B Rubout 30,6 50 0 121 36.8 - 0 119 in Vinvl 5 cuts 15 cuts 127 121 128 120 49.6 - 1.8 102 123 116 46.0 63 0 96 118 109 47.1 - 0 91 108 106 45.2 56.1 60,1 1.1 - 1.4 71 4,3 98 88 88 110 110 94 107 107 101 DUP050081281 4 Additional support for the proposed mechanism comes from the observation that the crystalline crudes used for pre-milling, which show surface areas of about 25 to 35 ms/g., are broken down in the milling operation to a nearly amorphous state of fine particles which are highly aggregated as shown by electron micro graphs, Proper breaching of the high energy particles with various solvents yields crystalline products ranging in surface area from about 65 to 75 m*/g. Solvents of higher potency were found to give products showing'higher v.p.'s and % 8 phase content as illustrated in Table 2 for products derived from the same pre-milled crude. TABLE 2 Breaching Solvent ODCB Perclene CCl4 v .p . 59.8 50.6 42.8 % B phase 12.6 4.1 0 Reference 1869/12A 1869/44D 1869/12B The postulated mechanism of breaching is in agreement with the mechanism of breaching suggested earlier by K. Batzar and A. R. Hanke for polychloro CPC. However, unlike the behavior of polychloro CPC, semichloro CPC is not entirely phase stable, as is shown in Table 2, particularly when the breaching solvent is relatively potent and the chlorine content is not strictly con trolled. Typical pre-milled plant lots from past production cam paigns show substantial variability in chlorine content (Table 3) with some lots falling below the specified limits of 3.8 to 4.5%. TABLE 3 Lot of Pre--Milled Crude 773 848 851 852 856 865 893 896 % Cl 4.3 2.9 2.0 3.6 3.9 4.1 3,4 3.8 In addition, the uniformity of chlorine distribution, al though believed to be significant, is largely uncontrolled. Mass spectrographic analysis of a purified semichloro CPC containing 4.5% Cl shows the presence of two substituted CPC's? a mono and dichloro species of unknown ratio (monochloro CPC requires % Cl * 5,81). Since the semichloro CPC is prepared by the addition of a specified amount of 4-chlorophthalic acid to a phthalic anhy dride charge, the effectiveness of mixing will have a bearing on the chlorine distribution (and possibly content) in the product which, in turn, will affect phase stability with respect to organic solvents. This problem has in the past been aggravated by using the same production vessels both for l c (chlorine-free CPC) and BB (semichloro CPC) interchangeably without cleanout in between. DUP050081282 -5 - To insure an adequate chlorine content in the crude, the amount of 4-chlorophthalic acid used in the synthesis has been increased and an effort is being made in the plant to avoid admixing chlorinefree CPC with the crude in order to maintain the required chlorine content. When using ODCB in the laboratory as the breaching solvent, substantial amounts of 0-CPC are formed even when the chlorine content falls within the specified limits. However, as is shown in Table 4, under essentially identical breaching conditions, the amount of 0-phase in the product increases as the chlorine content in the crude decreases. TABLE 4 Lot of Pre-Milled Crude 065 853 554 % Cl 4.1 3.9 3.6 % in Product Breached with ODCB 12.6 15.5 19.7 Reference 1869/12A 1869/9A 1869/8B Since the time of solvent-pigment contact is another variable which may affect the degree of phase conversion, it is understand able why the use of ODCB in the plant can lead to an uncontrollable generation of 0-CPC. Some plant lots have actually shown amounts of 0-CPC in excess of 30%, which; probably accounts for their ex cessive greenness and weakness. Thus, although particle growth is the mechanism by which breaching proceeds, the growth must be restricted and controlled. Excessive or uncontrolled growth can lead to weak products. In this respect, ODCB is not the solvent of choice despite its high degree of chemical stability in the basic breaching medium. 2. Desirable Properties of Breaching Solvents At this point, it might be in order to define the require ments of a good breaching solvent as determined in the present study. a. Ability to grow pre-milied semichloro CPC from very small, high energy particles without, however, causing over growth or excessive 0-CPC formation. b. Ability to form and maintain a reasonably stable emulsion in dilute aqueous sodium hydroxide by means of an emulsifying agent and reasonable force of mixing. c. Chemical stability in an emulsion with dilute (about 0.5%) sodium hydroxide. d. Possession of as low a boiling point or as high a vapor pressure as possible for easy and complete removal from the pigment by steam distillation. e. Non-toxicity and non-flammability. DUP050081283 -6- In view of the above requirements, ODCB is not an attractive choice for still another reason. Its relatively high boiling point (180-182C. ) maltes its complete removal difficult and time consuming even on a laboratory scale. On a plant scale# ODCB was left on breached pigment on numerous occasions, incomplete removal of the solvent maXes additional physical changes of the pigment possible particularly in the drying step (180*P.). changes such as additional particle size growth# phase conversion# and particle agglomeration are possible. in order to demonstrate these effects# two laboratory breachings were run on the same pre-milled crude using Staybelite as the emulsifying agent but one was deliberately worXed up without dis tilling off a substantial portion of the ODCB. The product from the latter experiment showed adequate strength by rubout but very poor dispersibility in vinyl both at 5 and 15 cuts on a two roller mill relative to the product obtained on complete distilla tion of the ODCB. The experiment was repeated with similar results. This product contained more 0-CPC and had a somewhat higher v.p. than the product freed of ODCB. Of greater significance# however, was the extensive agglomeration which occurred indie product not freed of ODCB in the distillation step. As is seen in Table 5# the surface area of this product was low and electron micrographs showed large agglomerates not unliXe those seen in the pre-milled crude although their crystalline nature was quite apparent. The fact that breaching had occurred was obvious from the v.p. and good rubout strength compared to that of the precursor pre-milled crude. ODCB Distilled Completely Incompletely V.P. 56.2 58.2 TABLE 5 Strength in Vinyl Surface of 5% CaSx LaXes % 0 Area 5 cuts 15 cuts 19.7 66 103 95 22.1 34 125 110 Reference 1869/5A 1869/5B The degree of ODCB emulsion stability is still another reason which puts ODCB at a disadvantage relative to other solvents studied. 3. Emulsion Stability Considerations Of the three solvents# ODCB# Perclene#and CC14# which have been studied in some detail# the first is the most and the last the least potent. This is apparent from the extent of particle size growth and a to 0-CPC conversion (see p.4). The more potent the solvent# the larger the ultimate particle size and the higher the 0-phase content in the product. Unexpectedly# when breaching under the same conditions of stirring# the product obtained on CCl4 breaching which showed the smallest particle size also showed the best dispersibility in vinyl. This is contrary to established principles. Obviously# another factor was at worX. In addition# it was shown repeatedly that the use of CCI4 in con junction with sodium Staybelite# used in breaching with ODCB# gave a product of poor dispersibility in vinyl. A closer examina tion showed that sodium Staybelite does not cause the formation DUP050081284 7 of a good emulsion of CC14 in dilute (0.5%) NaOH. Thus, to breach with CCI4, a specific emulsifying agent was necessary, but more importantly it became apparent that the quality and/or stability of the emulsion in which the breaching is carried out has a bearing on the ultimate dispersibility of the breached product. Thus, a specific solvent is most effective with a specific emulsifying agent which forms the best possible emulsion. Moreover, the solvents themselves in the absence of water, though capable of growing the initially small particle pre-milled crude and generating P-CPC in varying degrees, give products of unusually poor dispersibility (1869/3). It is obvious that in a regular breaching, the growth and conditioning of the particles occurs at the solvent-water interface, the extent of which depends on the quality and stability of the emulsion. To demonstrate this point more convincingly, the quality of emulsions of ODCB and Perclene using sodium Staybelite as the emulsifying agent and CCI4 in conjunction with Emcol P-10-59 were determined by taking photomicrographs of the emulsions as rapidly as possible after removal of a sample or, even more accurately,by the rate of settling or demulsification of the emulsions. Different quality emulsions, using the same ingredients, were prepared by conventional stirring and by high energy input in an Osterizer set at maximum speed. Breaching in all emulsions were carried out with conventional stirring. An examination of the final products dispersed in vinyl showed, without exception, for all three solvents, that breaching in an emulsion of greater stability yields a product of greater dis persibility. In addition, by comparing the three solvent-breached products with each other, it was obvious that CCl4 gives the best and ODCB the least dispersible product. This is exactly the order of the stabilities of the emulsion prepared with equal energy input. The stabilities of the emulsions prepared with high energy input and measured by the degree of demulsification in calibrated tubes over a 12 hours period are illustrated below in graphical form. The stabilities are proportional to the length of the solid lines and on an arbitrary scale are 72, 58, and 37 for the three solvents shown. Viewed in another way, the broken part of the lines denote the degree of settling of the three emulsions. CCI4 i -J- Perc ene ODCB ~r 1 1 58 I 37 1869/42 1869/44 ----1869/45 DUP050081285 4. Breaching with CCl* As had previously been shown by F. L. Reig, G-3300 was an acceptable emulsifying agent for breaching pre-milled crude with CCI4. In the present study, it has similarly been shown that the use of G-3300 affords good dispersibility products in the labora tory provided, in the absence of a laking operation, the acidextracted product is washed with dilute ammonia (1869/9C,F). The latter removes some dark base-soluble impurities. The removal of similar base-soluble impurities is of even greater importance when breaching with solvents in conjunction with sodium staybelite as the emulsifying agent. (See p. 15 ). CCI4 is a less potent solvent than o d c b and for this reason it consistently gave products of both lower v.p, and % 5-CPC as is shown in Table 6. TABLE 6 Pre-milled Lot 554 853 865 % Cl 3.6 3.9 4.1 Breached with ODCB 57.1 m. 19.7 61.2 14.7 59.8 12.6 Breached with CCl* V.P. 47.7 45.4 42.8 However, if the chlorine content in the crude fell below the recommended lower limit of 3.8% even CCI4 was capable of forming a small amount of 5-phase in the product. The low boiling point of CCI4, its ability to form good emulsions and yield p-phasefree products, provided the chlorine content in the crude was kept at a sufficiently high level, were important advantages in favor of using CCI4 as the breaching solvent. After laboratory and Semi-Works demonstrations (F.L.Reig) that CCI4 can be used as a breaching solvent when emulsified with G-3300, production was started in the plant. Although the dis persibility of most plant production was good, the performance was somewhat erratic and the products were red and dill vs. standard and at least the first 40-45 batches showed a substantial yellow migration in vinyl masstone (1% pigment). In addition, it was shown that the breaching tank was undergoing progressive corrosion. Expert opinion suggested that at the normal rate of breaching with CCI4, the life time of the breaching tank and associated equipment was only one to two years. 5. Dispersibility of Plant cci4.-Breached Products Unlike the performance in the plant, laboratory experience showed that product of very good dispersibility could repeatedly be obtained. However, even laboratory products were redder and slightly duller than corresponding products breached with ODCB. The redness could be attributed to the formation of less or none at all of the 5-phase in CCI4 vs. ODCB-breached products. DUP050081286 -9- Since pigment dispersibility was shown to he a function of the emulsion stability, an obvious question arose; what kind of an emulsion is being used in the plant? To answer this question, two plant runs using CCl* as the breaching solvent were followed close ly in a cooperative effort with Newport. The usual plant emulsion was prepared by recirculating the emulsion ingredients with a centrifugfal pump in addition to the ordinary slow stirring in the tank. The earlier described methods of measuring emulsion stabil ity showed the plant emulsions to be more stable than conventionally-prepared emulsions in the laboratory, but inferior to those made in an Osterizer. However, unlike the behavior in the labora tory, continued pump recirculation of the breaching mass during breaching appeared to cause or contribute to the breaking of the emulsion early in the breaching cycle. Following the failure of the emulsion, agglomeration of the pigment ensued which could be readily observed under the microscope. Simulation of this condition in the laboratory by using the same emulsion for two breachings but different energy inputs during breaching, caused the more vigorously agitated emulsion to break rapidly and yield a product of inferior dispersibility in vinyl (1869/53) relative to the product obtained on conventional stirring during the breach ing process. Once again, pigment agglomeration which occurred in the rapidly stirred emulsion could be observed under the micro scope and photographed. In addition, in one plant run, samples taken before and after breaking of the emulsion and worked up in an identical manner in the laboratory showed a definite dispersi bility advantage for the former. These findings suggest that the initial emulsion should be made with the greatest energy input to form as stable an emulsion as possible, but after the introduction of the pre-milled crude, the breaching be carried out with gentle stirring to avoid breaking of the emulsion. These changes were immediately incorporated into the process to the extent possible with available equipment. The results were quite satisfactory. 6. Migration in Vinyl and Hydrolysis of CCl* Although good dispersibility in vinyl and strength by rubout are important requirements of BT-449-D, the pigment must also be free from migration in vinyl. Thus, any solvent or emulsifying agent used must not lead to substances in the pigment which will cause migration in vinyl. Still another important requirement of the breaching system is that it not be excessively corrosive to soft steel, the material of construction of the plant breaching vessel and associated equipment. The cause or causes which led to migration in vinyl and corrosion of the equipment when breaching with CC14 were not immediately apparent. At first, it was assumed that the emulsify ing agent G-3300 or its breakdown products were associated with the bleeding substance. However, direct addition of this agent to non-bleeding BT-449-D failed to produce migration in vinyl. To understand the possible effect of breakdown products, it became DUP050081287 - 10 necessary to find the structure of <3-3300. The producer of this agent. Atlas Chemical Industries, Inc., was reluctant to disclose full details concerning the structure. Based on partial suggestions of structure, IR spectrum, behavior with respect to base and elemental analysis, it was established that the agent (1869/13) is the isopropyl amine salt of dodecylbenzenesulfonic acid*. All salts of the sulfonic acid which could conceivably be formed and remain on the pigment, such as those of Cu and Pe+3 were prepared and incorporated into non-bleeding pigment* The added salts failed to show migration in vinyl. A clue to the migration as well as the corrosion problem was discovered when it was shown that two breachings of the same pre milled crude with ODCB and CCU in the same initial concentration of sodium hydroxide gave filtrates of different pH's at the end of the breaching procedure as shown in Table 7. TABLE 7 Breaching Solvent ODCB CCU initial p H 13.0 13.0 Final p H 10.0 8.8 Reference, 1869/9E 1869/9F Although a decrease in pH was encountered with either solvent, it was repeatedly shown that the decrease was greater when breach ing with CCU* A test for chloride ion in the final filtrates from the ODCB and CCU breachings was negative and strongly posi tive, respectively. It was obvious that CCU was hydrolyzing under the conditions of breaching* A review of the literature disclosed** that CCU hydrolysis in aqueous mediumwas known and that the rate of hydrolysis is second order with respect to CCU and is independent of hydroxyl ion and chloride ion concentration. It was clear that during the breaching operation, NaCl was being generated in the basic aqueous phase and HC1 in the vapor phase, CCU + 4Ha0------4HC1 + C02 A close inspection of the plant vessel has actually shown a greater degree of corrosion above the liquid level than below^it as might be expected on the basis of the effect of HC1 vs. cl" on mild steel. The extent of CCU hydrolysis in the aqueous phase could be ascertained by analyzing the final filtrates for chloride ion. Some analyses are given in Table 8. Based on the identity of IR spectra, behavior toward base and effectiveness in breaching it was shown that Emcol P-10-59, produced by the Witco Chemical Co., is identical with G-3300. The former is used extensively both at Newport and Newark and is less costly than G-3300. This information has been transmitted to Production, **I.Fells and E,A.Moelwyn-Hughes, J.chem.Spc. 398 (1959) DUP050081288 - 11 - TABLE 8 Breaching Solvent QDCB CC14 Concentration of Cl* in cr/1, 0.029; 0.038 2.57? 2.74 Reference 1869/46 1869/42 Since tap water used for breaching contained 0.008 g/1 and the ODCB filtrates showed 0.03 to 0.04 g/1 Cl ion, the difference arising most likely from impurities in the other breaching ingred ients, the hydrolysis of CCI4 generates (2.65 - (0.033-0.008); about 2.4 g/1 of Cl** ion in the relatively short period (2-3 hrs.) of a laboratory breaching. The concentration of generated Cl"" ion in the plant was probably higher because of longer contact time, at high temperature/between CCI4 and the aqueous phase*. The occurrence of corrosion appears to have been directly linked with the migration problem. Many different pre-milled lots breached in laboratory glass equipment failed to show migration in vinyl. It had to be concluded that the corrosion of the in terior of the plant vessel was somehow involved in the generation of the bleeding impurities. In addition, it was shown that migra tion of plant CCI4 breached products became progressively less pronounced as the number of runs (about 45) increased although migration did not disappear altogether. It appeared likely that the corrosive effect of Cl"" ion on the wall scale which had accumulated over two decades of operations, as well as of the mild steel itself was giving rise to the migrating substances. Although the migrating impurities were not identified, it was shown that a standard CC14 breaching in a steel autoclave yielded a product which showed an unmistakable migration in vinyl. When the tempera ture of breaching in the autoclave was increased, the degree of migration also increased (1869/23). Upon adding some of the scale collected from the Newport vessel to a standard breaching in the steel vessel, a product was obtained which showed a strong migra tion in vinyl of the same color as encountered in plant production. Thus, the causes of corrosion and related migration have been identified. The excessive dullness of plant CCI4-breached products may have been, at least in part, due to the generation of the migrating substance. It was clear that CCI4 could not be used as the breaching solvent for the production of BT-449-D. 7. Perelene as Breachho Solvent A new solvent for breaching which is more chemically stable than CCI4 but less potent and lower boiling than ODCB, and one which forms satisfactorily stable emulsions had to be found. Several solvents were tried. Chlorobenzene in conjunction with sodium Staybelite gave a product of lower 6 phase content relative to ODCB (5,2% vs. 14.7%) and a lower v.p. (58.6 vs. 61.2)(1869/10) *A plant-breached mixture (X-25) taken prior to CCI4 distillation and stored at room temperature in a five-gallon kit for about six weeks showed a drop in pH from 11.8 to 2.5 and a very strong positve Cl" ion test. DUP050081289 - 12 - but also inferior dispersibility in vinyl. Methylene chloride is far less potent than ODCB, but more potent than CC14 in terms of 8-phase generation and particle size growth despite its low boiling point. Although considerably more hydrolytically stable than cci4 (1869/46B), its boiling point is much too low for handling in a plant operation. Tetrachloroethylene, Perclene, was found to have a combination of physical and chemical properties including its ability to form adequately stable emulsions in dilute NaOH which made it a solvent of choice for the breaching operation. Its chemical or hydrolytic stability was found to be sub stantially greater* than that of CC14 and essentially equal to that of ODCB under the conditions of breaching. The greater hydrolytic stability of Perclene was apparent from the degree of lowering of the pH on breaching of the same pre-milled crude with CCI4 and Perclene as shown in Table 9. TABLE 9 Breaching Solvent Perclene CCI4 Initial pH 13.1 13.0 Final pH 11.3 9.1 Reference 1869/44 1869/43 Breaching of the same pre-milled crude with the various solvents gave concentration of Cl" ion in the final filtrates shown in Table 10. TABLE 10 Breaching Solvent ODCB Perclene Perclene** CCI4 Concentration of Cl** in q/1 0.034 0.041 0.044 2.6 Reference 1869/44 1869/45 1869/58 1869/54 Perclene clearly shows a hydrolytic behavior similar to that of ODCB under the conditions of breaching. In addition, the boil ing point of Perclene is 121C., about 61 lower than that of ODCB making complete removal of the former from the pigment considerably easier. As a solvent for CPC, Perclene is considerably less potent than ODCB but more potent than CCl4 as judged by % 8-phase content and v.p. of laboratory-breached products derived from the same pre milled crude at pigment to solvent ratios given in Table 11. * According to Elchera, under a specific set of conditions, Perclene is about 2000 times more stable than CC14 with respect to hydrolysis in water. **Semi-Works run 00272, DUP050Q81290 - 13 - TABLE 11 Breaching Solvent ODCB Perclene CC14 Picment/Solvent 1.92 1.53 0.63 %JL 12.6 4.9 0 59.8 53.9 42.8 Reference 1869/12A 1869/44 1869/12B A study to determine the optimum amount of Perclene to be used in the breaching operation gave best results at a pigment/solvent ratio of 1.23. The amount of Staybelite found to be satisfactory was 7.5% based on pre-milled crude which is 1.5% above the minimum required for optimum dispersibility (see p.15) Using these conditions in laboratory breachings, products of very good dis persibility and rubout strength were repeatedly obtained. A Semi-Works run (00272) based on laboratory determined optimum conditions and using a powerful recirculating pump for the emulsion preparation and a flash distillation unit for Perclene removal gave a product of very good dispersibility (superior to standard at 5 and 15 cuts in vinyl) and superior rubout strength (about 1.2% stronger) without requiring laking with calcium Staybelite. The product contained 2.9% 8-phase and showed a v.p. of 51.6. Despite the higher amount of Perclene, the differences with the data given in entry #2 of Table 11 (products derived from same crude) are probably due to the short pigment-solvent contact time at high temperature in the flash distillation unit compared to that of a conventional laboratory batch distillation. The semi-works product was slightly redder but just as intense as standard. Using Staybelite as the emulsifying agent and Perclene as the solvent/ it has been shown in the laboratory that the pre-milled crude must show an extracted solid purity of 85% or higher. The lower purity pre-milled crudes cause early breaking of the emul sion with consequent impairment of quality. Although the nature of the impurities is not known, it has been demonstrated that in organic salts will either decrease the stability or cause the emulsion to break. The reason for breaching in about 0.5% sodium hydroxide is that doubling the concentration (increase total ionic strength) in carefully controlled experiments had an adverse effect on quality, presumably due to a lowering in the emulsion stability, Other substances such as NaCl or alum (1869/36), the latter could conceivably be an impurity in pre-milled crude, were shown to have a similar deleterious effect on emulsion stability. 8* Perclene - Emcol P-10-59 Combination Unlike the other solvents studied, Perclene is unique in that it can be successfully used for breaching with either Staybelite or Emcol P-10-59 as the emulsifying agents, the latter forming the better emulsion under the same conditions of agitation. DUP050081291 * 14 - The greater stability of the Emcol emulsion was demonstrated hy a comparison of the settling rates of two emulsions prepared with an equal concentration of emulsifying agents and power input. Below is given a graphic comparison of the emulsion stabilities. Perclene/Staybelite Perclene/Emcol T 75 1869/44 1889/23 The Perclene-Emcol combination gives the most stable emulsion. In agreement with this finding, marginally pure crudes (less than 85% purity) gave products of substantially better vinyl dispersi bility when breached in emulsions prepared with Emcol P-10-59 rather than Staybelite (1889/23D). In addition, variation in the amount of Emcol used per unit weight of pigment causes less fluctuation in quality vs. similar changes in the amount of Staybelite (1889/ 19,21). Unfortunately, the ability of Emcol to form stable emul sions creates problems in filtration of pigment from basic solution which is the new mode of pigment isolation using Staybelite as the emulsifying agent (see p.15). Since the Staybelite process, as presently modified, is more economical and produces good quality product, there is no need, at present, for an alternative agent. However, should the need arise or should a better method of fil tration be devised, Emcol could be considered as a possible alternative emulsifying agent. 9. Plant Breaching with Perclene After the successful demonstration of the Perclene/ Staybelite process in the Semi-Works, manufacturing was started in the Newport facilities. Although the stability of the Perclene/ Staybelite emulsion produced in the plant was not as good as the DUP050081292 - 15 - one prepared in the Semi-Works (a more powerful pump was used at Newark) nevertheless in a ten batch campaign, seven batches showed vinyl dispersibility and rubout strength within shipping limits . The intensity of the products continued to be deficient relative to standard. In an effort to learn more about the process and ob tain more consistent performance and improved intensity, several plant batches were followed closely in cooperation with F.L.Reig. It was shown that "in-process" samples including those taken prior to pressing worked up in the laboratory were in most cases stronger and more intense in vinyl and by rubout than the corresponding Newport lots and essentially equal to the quality of the Semi-Works product. Since the final steps of the process call for acid ex traction followed by pressing, acid-free washing and press washing with dilute ammonium hydroxide, it was suspected that the final alkaline wash, which in the laboratory is known to remove Staybelite and other base-soluble impurities was not very effective in the plant. This was confirmed by demonstrating a significant improve ment in quality upon extracting plant lot samples of inferior quality with dilute sodium or ammonium hydroxide, the former being more effective. Well base-washed or base-extracted products (1889/12) showed a 1.5 to 4.0% lower Staybelite content relative to the plant press-washed counterparts. In addition, it was shown that failure to base wash yields a product with a surface area of 50 ma/g while an effectively laboratory washed or extracted counterpart showed a surface area of 70 m/g (1889/12). Thus, ineffective plant press washing leaves behind impurities including Staybelite which have a deleterious effect on dispersibility and intensity of product. While washing of the acid-extracted product with proper press loads presents no problems, subsequent washing with dilute ammonia appears to reactivate the Staybelite present on the pigment causing the latter to peptize, and changing its washability characteristics. Channeling in the press is not an infrequent occurrence. Since proper press washing on the basic side appears to depend on the amount of Staybelite used in the breaching, an attempt was made to reduce the amount of the emulsifying agent. Unfortunately, substantial reduction of the Staybelite amount (1889/19) lowers the stability of the emulsion and causes a drastic decrease in the dis persibility of the product. The minimum amount required was found to be 6% on a pigment basis. Since the process calls for 7.5%, drastic reduction of Staybelite is, therefore, not possible. One way to remove alkali-soluble impurities which unlike the press washing does not depend on chance, is to reslurry the acid- free washed presscake in hot dilute (1%) sodium hydroxide and carry out a bona fide extraction (1889/12F). The effectiveness of this approach has been demonstrated both in the laboratory and in the plant (plant lots X-12 through X-17). A closer examination of the plant process, however, shows that a more effective way to remove base-soluble impurities is not to precipitate them on the pigment by acidification in the first place and subsequently attempt a basic reextraction, but rather to press directly after steam dis tillation of the Perclene while all impurities are in basic solu tion in which the pigment is suspended. At this point in the process, the base concentration is slightly under 0.5% and can be DUP050081293 - 16 Increased to any desired level (1% is sufficient) and by heating nearly to the boil, any remnant of solvent can be eliminated and, in addition, the filtration facilitated (F.L.Reig). In the labora tory, this process offers no difficulties, in the plant, some difficulties of pigment bleed have been encountered particularly when applying high water pressure during the washing cycle. How ever, with manual wash-water pressure control, the last BT-449-D campaign (see attached batch card) was the most successful to date in terns of vinyl dispersibility, rubout strength, and intensity of product. Ten breaching lots from Newport were combined into eight acid extractions at Newark using about 1/2 lb, of HgSO* per pound of pigment. The results are given in Table 12. The only problems encountered in this campaign had to do with yield and lot identity. It is noteworthy that the base-extracted material shipped from Newport does not settle in the drums and consequently does not require extra handling at Newark. Plant Lot 56370 58406 56455 56625 56794 56889 56926 56970 TABLE 12 Yield of Ground Npt.Lots Est.No. Pig- % of N--13 of # raent Yield 46-48 2360 1775 75.2 43--44--450 1422 1427 95.6 45A-45B 2049 1862 90.9 49/52 2322 2340 100.8 50A/54 2151 1155 53.7 51/50B/54 2300 1341 58.3 53/50B/54 2300 47A/47B/ 1936 84.2 47C/54 2300 1826 79,4 Vlnvl Dispersibility, Rubout* 97Rh 5 Cuts 15 Cuts 92 96G^IA5 98R4D4 115 103R13D20 100R8D8 99 98 I18 99RA5D1? 110 lOOR^D2 100RXOD/U 97 90R13 93R12D1^ 95 90R13 93R10Dl3 100 96R10 93R6D10 100 95R10 17274 12662 79.2% Relative to standard lot 97419 The slight dullness shown in rubout requires comment. As stated earlier, breaching with Perclene yields products containing less 0-CPC than the ODCB-breached counterparts (standard is ODCB breached). A- a consequence, Perclene-breached products can be expected to be redder. It has been shown that the human eye tends to associate redness with dullness in CPC colors. Thus, blending of a BT-449-D sample breached with Perclene, which was read by Quality Control 96R12D12 v s . standard, with *1% 0-CPC (BT-383-D standard) has given a product which was read 97Gl3-e vs. standard and lOOGiailS vs. the original BT-449-D sample (1889/27). There fore, products from the new process can be expected to be somewhat redder and slightly duller vs. standard by rubout. For this reason, in the following campaign, products will be collected for setting up a new standard. After a new standard is set-up, products produced by this process can be considered for conversion to other existing codes such as Bp-173-d , BSP-425-D, and BT-413-D. dc DUP050081294 M' Oor.- K< j R.:.. " . .tj ...... 0` :*. ! ^REACHING >...4 ;: Rev. 3/21/68 XOP- l4oo,; s ize: - 4 {Fordone IVryachinij; '* Caustic Extraction) - Xnntruo. tionu * ' iv -t t "~'r" CnWXOITl ADD PROKiR CHEMICALS IN CORRECT ' AMOUNT'S AND StlQUEEJCS TO ELIMINATE .i lAf.'i.ADS t, 1. Check C:> Still.: Should be MT > Min. Mex-j '). Aciii ;/&t,cr to still, start agitator. / Start, reel i4 evict inf. (2n valve open). Check .ryeire.uleting line working. Supervisor must be present. 74" 7-5' 4. Add 3 pots oi' f>0# con Stic solution {15 . IAlC.) 3 fo' ). A;Utar.c for 1/4 hour. 6. . h ir^k pH of still contents 'in fry. vq-n^f. t-n -U.vrsO. if_ruKS^sa:ry. '.!: .5-13.01. f pr **mfief pH IX, / 13 . o 7. Close still manhole. Check -j see that vapor- .line valve is closed, and irater is on condenser. ;j. Vi It'a agitator on, add 3taybclite/J?erclene10^/23'' i, Close 2`r and. open fcy-pass through <: ri f i co ; j /?." ). Rec 1 rculate 2 hrs. r h TS . 10. Sarnie X FT omuls5.cn at bottom of still. tilvis to Supervisor. Must pass k-minute stability test. n. Before charging pigment, close by-pass % valve and recirculate through 2" line again or. in Step 3- Charge- 14003/pretnill.cd BBS (lb hrs,) o>r>; a one-hour period. {.Approx. 1 Drun/9 mins.). 1400/ V Lot # Lbs. 7- v J 3. A'itete and. circulate for 1/2 hour. Ln-vliC 1 flL at bottom still valve, wive to supervisor. Must pass 5-minute stability teat. DUP050081295 k'r- V i_____ jit. ! ! ; I | ! i Xu.. i Instructions ..lii Open lvv-pa,-.r. steam twoturns. j * v:'fn\ still temperature-' reaches 40*0.! <:. oso by-puts :;tean vi'.lvy, Stop rec.1 r- i Uiun.;- rluwh rc.ircu3 atine; lino ami I v.-v t.--Aisn with water, ; 'i Open valves i`o.vautomatic'steam control, j Vi.r:;temperature to pO-b.V'C and hold for ! 2 urs, ! .i rttUra;:- { ' l .-' /> ) ... ;: iiv' v ': {. ;:;; : dc 7 7: /Hi' 1H$ -.. I IV. fxf tvr thn 2 hours .breaching, close steam valves to 28 still/jacket, $Sako sure maximum 'water is on conueneer. Cross connection to peerless pump line mat be open.- l3. Check 4/R tank If]1,, ; j; j m. r'i v :dB,> - V-'A'.-. -!> i:W: i 19.. Add water to flush still' Accumulator with manual by-pass ('3rd Kir. ) valve to iyO'Jv of chart. Set LHC-10. on auto matic-control at this point. ' ' , i 20. One-half hour before hold period is tip, turn steam on flash still very gradually to X3~80$* of chart for 1200 .11?%/hr, steam. This will heat up all pi pan before dis tillation, Set valves to' return cond.cn- ' sate to outside decanter... (Check rota- : meter for flow during heafcinc up). 1 i . . a ! . ? ' i - ; 21. Open remote operated water valve (con- j tains 1/3". orifice) to accumulator, i Adjust FRC~9 manually at psic ' air to valve) to drop 2?.'- still level | about 10"-18"/hr. If dice,illation is j interrupted for anyjcfeaso.n ~ close remote operated water valve to vbe accumulator i- and leave closed until ctiv.fination feed : i s resumed. THIS IS IHPOkTAkf or c>xccr>s5ivo| water will accumulate in i:7'i tank, ! 'i: 1 . 22 ; I I Check the distillation every hour and roc ora. 'the followirii; information. If the accumu lator level begins to rise near the end of the cycle., reduce' -feed `rate to hold con stunt y Start 4715 agitator when 4YB level reaches ; 36" - \FCm:~* 4.7; A i a, tor -'.'w. :T > - v ; / '. ;7 " i: DUP050081296 ........... ............ j p I'v.o'-rt data every hour. ST1U, POT ~ ' V . iFUSH^cnTx.""* ; -------------------------------- --------j: Foci} XJU./fir. :Steam tYd *TTT finoj Level Tenr>-*'C. j FOR-9 IFCH- } Level l ___l ':....1. ........................................ !: ij i . .( >i ...................... ! j L____ i-- L ...____ i . .. 3- When distillation is nearing completion, a low level alam \?ill sour'd indicating, low level in 28 Still. ! 24. Continue tint11 28 Still is empty. Close still outlet valve. .Plush FV-9 valve j and flash still with- water, , ) j j 25. i:<'. FJJC-y rKU'ually at 0 air' output to ( close feed control valve. i 26. Wait 5 minutes3 then turn off stem; valve FV-3. i ! | | j 27. Add 3 pots of 50% caustic solution, then j t add water until level indicator just moves ; and purip directly to tyii by-passing j flash- still. . 1 ? 28.. Drain accumulator by opening FV-XO j (lower set point to 0). ..Flu ah with manual ' by-pass xjater valve to 30# and drain again.* Close remote.operated water valve(3/16" orifice) to accumulator. j 29, Close still outlet valve.' 30, Close high pressure steam v-uce outside The distillation cycle is complete, pirSri font. Have iecR filterability of sample, lo t # Level and pH Temperature Time . ' |On Batch Card ax'd Cample label). ; i* 7 ' :u. t - i .j 1 : ? i ': i DUP050081297 Si i\ i &sp ! ii ki ft ' Vs F- i 7i I V kI H XOP- ' JU . Instructions r.cohock and record pH in lab froir- 4yji recirculation line. Should be 11 3-13. /-;V;uri: Xi' less than 11,3 r;/?rc or r0>.'> cauatic .and recheofc pH. mated Total 50$ Caustic "C?o~:`Sestrcd/liT'KaOfr SolTJ'ion at *V?B) K'X level >y( 30 3 y3i r,n M /j 6,j Total 50# C n un tic 31.5 Gallons 32.5 34. 5 36,5 35.5 40.5 4h.5 Addit at'4?: Lbc.. ~Q 16 29 Vj SH U to d If you one11 Perclone in the o .m notify supervision. Chock agitator on and beat to ;o*C, Agitate 1 hour nt 90- 95C. .... PRESS OPT (4? PRESS) --------- (32 Prams) i. Chech 57 press, clean and. iff/ Set rp recovery system. Puns*? charge to SI press, fill precis, Check tank MT.',...... Tank is MT,. (Supervisor's initials) u) Hta .rt uu sh i ng. 10-15 4. Wash lor 6 hrs. at / psi water -pres sure vrith vans (4QC) water. At the end .1 0 hrs. chock filtrate in .hit* for pH. . IF i"' 'ii . iiij)|,g** pH is high~ain.ni ,iiu:Uo4'i tc ptn-ii i{^ continue to wash and re- canipie every hour. !3- Record total lire, washed, Pine.X-^ . Ohms -... . -- ~ pH c CH*e* to Mia f a MT >#w rS4-4 gh'oel^fcu' TTWi 7, Dump.ureas charge to fafWWt* rresscake full, firm or sloppyv If prcsscake smells of Fordone, inform- your suoervloorl Vrf5 . 1 *! VI .. t- \ : 'X ! ' - DUP050081298 r i: i Ot *;" i I i ; i ! i ,9 ? ( ! I U!"" " r* i , t fit : /* i j n* V .< J r-i : ' ,:j .. /'\(n fir.< u>n t Chr < > ." i:-;.. pr..... `. iv.-.'t W .' vi. 'inci raj.-V. ! V- .'. *_'r .*;*> -I ta.'.f b<i CJir .1 .I :'n ..Cu;:, V. i: '< *.* I >-Jr. t). i rU- roc-v*. Mmt*+ n* **<*- a m? St;...'', artxronins Tret?- riS.xe*\ . - . Tata; v.rj - 1 <$fc. sartpleo vrhiio pad; in cu; . ' -CcU.uctv.ono dipper.fron feed cd caon drum dr;on drurt Ir. approximated' 1/V. .full. fi<v;crd!; f.ot No.. ... __ _______ _______________ lie. of Wot Pv ana' . Vy .v., Ho, of PrnruB Wot &;v^. t ; oil - f** : Total Wot. Wet.______________ /V, N J.3-A-, lot, net and tare , . .,* ;.* r.." mV) each drv.si. 71- d. nixer arm rccirculIvne ; -jiv: vrutirJ;s^i.v_i!own sia-tii,.' I MAKEUP 07 >y.WYnK/;r:i::. SOfAfflOW (For one batch) ! To nix tan!; on 3rd floor .add 3,` ( :>' ;'.al3...).. pyrelonii.^__Tube sample of ! Pcfv.'fono to- J.ab for upeeirlte rnivi i" ; Civ?ok.; Rehora epeciflc; ^ravily bore-;- - ;. | (>> ; / i-.aa 'f u-W .?.i* crwjsfied Sva/be li be. St; r for at., least.. 30 il road:/ for cUarr.in Wo3 `1 l.,, ............... iii ,. --- DUP050081299 New Jersey Office Supply Co. Filing Specialists 401 Frelinghuysen Ave., Newark, N . J. 1 2w C aX DUP050081300