Document k6MXXXVZrgqjNe4w8EeymbQrV
IWARY 1976
lootings form effective barriers
in PCB-contaminated silos
| t. B. WIUETT
I** The polychlorinated biphenyls /(fcn'l) have been vnlunble inclusj. trial chemical* whir It have hern j uwtl extensively in many products | since about 1930. However, in
1966, PCB't were identified as en vironmental contaminants which are persistent and tend to accumu late up the food chain. The pro duction and industrial use of PCB't have been curtailed in re cent yean; however, PCB's can atilt enter the environment from mnteriab containing biphenyls.
One aource of PCB's entering the human food chain h a coating material called Cuntar for concrete silos. More precisely, the coating .contained the PCB's called Aroclor 1234 (Monsanto). It was used between 1941 and 1970 by several silo fumpanic* in Ohio and neigh boring slates. The PCB's from the Cumar silo coating are dis solved by the silage juices and PCB residues migrate into the silage. When the contaminated silage is led to cows, the PCB residues ac cumulate in the body fat and are excreted in the milk. The Food anti Drug Administration (FI7A) has established a "temporary toler ance" for PCB's of 2.5 parts per million (ppm) for milk on a fat basis. If this tolerance Is ex ceeded, the milk can no longer be
marketed. In 1971, after the silo coating
was identified as the source of PCB-contamlnation, a research program was initiated to develop methods of decontaminating silos
?reviously coated with Cumar.
reliminary laboratory studies dc
l.. S. Wlll.lt It ItlMirM p,ltw>. OsiwtilWtt t Dolly fcltitcs. Ohio Agikvl'
h*#l Ktltoith cinrt Dovolopm*n Cmtor.
termined th.it various coating tn.v tennis would form harriers to PCB mulue*. The coatings which pro vided the most effective harrier* to the residues in laboratory tests were then applied to dairy farm film known to lc contaminated.
Preliminary results of these trials were very' encouraging. The barrier coatings effectively reduced the residues appearing in the silage. However, these results did not in dicate whether the barrier coatings would be effective when the silo 'was used continually.
Study of the effectiveness of the barrier coatings on the earlytreated silos has continued. Addi tional silos have also been coated. Table 1 summarizes the average concentrations of PCB's in silo wall scrapings and silages collected be fore and after treatment with a barrier coating. All of the silage samples were collected adjacent to the silo walls at approximately 2week intervals.
Silos 1 and 4 were both cleaned by wire brushing the wall surfaces and recoating with hydraulic ce ment containing an acrylic bonder (Thoroseal and Acryl 60--Stand ard Dry Walt, Inc., Miami, Fla.). Silo I has been filled alternately
with grass and corn silages a total of five times. Silo 4 has been filled twice, once with grass and once with corn silage since recoating.
Silo 2 was cleaned with high pressure water (500 pst), then re coated with Waiter-carried epoxy (009 Epoxy--Action! Plastic, Inc., Charlotte, NIich.). The top 13 feet of this silo remained unronted. The silo was filled four times with corn silage.
Silo 3 was also cleaned With high pressure .voter and then rccoated with furfiiry) resin coating (SileniCrete--Universal Cooperative*, Al- '
linnee, Ohio). This silo \va half i
Filled with grass silage. When the , grass silage was emptied, the ii)o was filled with com silage, then re filled with gran silage.
Silo 5 was cleaned by brushing the wall surface* then re coating with a water-carried epo designed to give a "high build" ge ; thick coating (009-900 HB epoxv --Action! Plastic, Inc., CfcartatrMich.). This silo ha* been Elrr twice with com silage.
Silo 6 was constructed of waxed staves, therefore, sandblasting was required as a cleaning method. This silo was coated with a poly ester coating (KanGlas--Feller Enterprises, Inc., IVaukon, Iowa).
This silo was filled with grass sil age, partially emptied, and then refilled.
All of the barrier coatings used on these silos have provided an ef fective reduction in the concentra tion of PCB's in the silages and have maintained their effectivenesa with continued use. The use of trade names is to identify the prod-
TABLE 1--.Effectiveness of Bar-, risr Coolings.
Silo 1
&<o 1 Silo 9 Silo 4 Silo S Silo 0
SlfOpiftft Sitofo* Sllofo*
brBf koioro
oflor
moolltay totooHng
Port* pH million (ppm) of Kfi
JO. 133 3*0 364
>10.000 33.503 391
7,137
33 183
60 130
30
0.1*
Vttt 1.33 0.1* 0,7$ 0.M
'
MONS 08733/
OHIO REPO4
ucU used in this rrv*rch u..J is
nol in milnrumrni of these prod ucts nor meant to discriminate against similar products not tinted.
The hydraulic cement coating was the most effective material. The average concentrations of PCB residues in silages from the hydrau lic cement-coated silos were about five to six times lower than from the silos protected with epoxy or furfuryl coatings. However, all coatings reduced the PCB's in si lage sufficiently to keep contamina tion below the actionable level.
The "high-build" epoxy and polyester coatings have not been evaluated for as many seasons as the other materials. Both appear to be promising materials. The "high-build" epoxy shows a marked improvement in effective ness over the other water-carried epoxy. The polyester appears to be as effective as the hydraulic ce-' men! and will continue to be stud
ied. The coatings have remained
well-bonded to the silo walls. Bonding has failed in only two in stances. A small area (approxi mately 3 feet by 3 feet) of the coat ing In Silo 1 came loose after four fillings. A similar area of the coating came loose in Silo 3 after the second filling. These failures probably resulted from insufficient cleaning of the silo wall in those areas before the coating was ap plied. In each case the area was easily repaired hy the dairyman.
It has been determined that dairy* cows deposit between 11 and 2? percent of the PCB's they con sume into the milk. Therefore, under most dairy feeding system*, Ihe concentration in silage adjacent to the silo walls would need to ex ceed 5 ppm (dry matter basis) be fore the "temporary tolerance" ' would be approached. The etfec4t(vrnem of the harrier coatings has ; Wen further verified as the PCB
Concentration* In milk produced I the farms with these silos have
nil declined below the "tolerance
level. A dairyman who owns a silo
which was once coated with Cumnr and is PCB-contaminated may wish to use the barrier coating ap proach to eliminate the residue. In many instances, barrier coatings are more practical than removal of the silo considering time, expense, and convenience. However, if various barrier coatings are to be effective the following considera tions and precautions should be observed.
I Tf a silo is to be decontaminated
by recoating, dirt and loose par ticles of old coatings and/or de teriorating wall surfaces must be removed. The barrier coating will be no better than the surface upon which it is applied. If the silo is tn very poor repair It probably will be best to replace it.
Sandblasting is an excellent me thod of cleaning a silo wall sur face upon which a new coating t* to be applied. When this method is used, care should be taken to control the dust, debris, and sand which can spread PCB contami nation to other areas of the farm. The expense of sandblasting makes this approach impractical under some circumstances.
Washing the surface witli highpressure water (500 psi) has been shown to be an effective means of cleaning silo walls. When this me thod is used, the runoff must be controlled to prevent PCB con tamination of waterways. Time must be allowed for the silo walls to dry prior to application of the coating. Therefore, some delay must be expected when water is used. This is particularly impor tant in the winter when frost may build In the silo walls, preventing good landing of the coating.
Wire brushing of the silo surface is also effective, but requires a great deal of time and lutar.
A special problem is presented in preparing to recoat a silo which
still has a previous mating intact.
or was constructed of wax-treated blocks. Unless the old surface b removed or a firm rough surface prepared, the chances of good landing of the new coating are
greatly redured. A coating sh--hf
never be removed with an organic solvent because It will spread tkt
PCB contamination and may lone the surface unlit for rerouting;
With solvents, there is also the dan
ger of fire and/or toxic vapors.
Sandblasting may be the best wap to remove ait intact coating.
.The coating used ns a barrier lo PCB's must withstand the hands
environment inside a silo, plus pea-
vent the acids in silage juices from
reaching the silo wall. Some of
the desirable coating properties art
listed below.
-
(1) The coating must tand weft
to concrete.
'
(2) The coating must be water proof, non-porous, and cover com pletely.
(3) The coating must be aeh^ resistant because pH values as low
as 3.5 are encountered.
(4) The coating must withstand
temperature ranges from below
freezing to 160 F without failure.
(5) The coating should bn
tough m that machines,, such aa
imloaders don't cause it lo flake
off.
(6) The coating should not coo tain chlorinated hydrocarbons or
toxic chemicals which will con taminate the silage. FDA ap
proval of the prcduct for feed con tainers is recommended.
(7) The coating should meet
Occupational Safety and Health
Act (OSHA) standards to protect
the workers applying the material
from toxic or flammable vapors. The product mint also meet local air pollution control regulations. .
(8) The coating should not con tain a solvent in which PCB's am readily soluble because PCB's from
the silo wall may migrate Into tfcfe new coating ns H is applied*`
"T* -f- *
<>
MQMS 087333