Document jyLn1528KpndvNGw2ydpmrL32
E. I. DU PONT DE NEMOURS & COMPANY
256 VANDERPOOL STREET NEWARK, NEW JERSEY
Serial No. KN-69-9 Copy No.
NEWARK PLANT PIGMENT COLOR RESEARCH REPORT
STUDIES ON THE IMPROVEMENT IN HUMIDITY RESISTANCE OF INORGANIC AND ORGANIC PIGMENTS IN '*927" ACRYLIC LACQUER
Period Covered November, 1968 - July 15, 1969 (Part time)
FILE; 173
DATE:
7/23/69
NJ 14071
DUP050081467
KN-69-9
1. Numerical File 2. Research Office File, Newark (173) 3. Newark Library File (173) 4. M.Hunt/E.Gonick, Pigments, Wilmington 5. W.S.Struve 6. F. F. Ehrich/H. H. Gyorgy/B, H. Perkins/Newark Libraary 7. P.j.Monahan, Newark (Vital Records) 8. N.6.Fisher, Central Research Dept., Wilmington 9. R.H.Wetzel,/Newport Research File 10. J.F.Maurer/J.W.Minnich/W.A.West, Newport 11. J.Jackson 12. W. J .McClure/R.A. Hageman, Newark 13. Extra 14. Extra 15. Extra 16. Extra 17. Extra
NEWARK PLANT PIGMENT COLOR RESEARCH REPORT
SUBJECT: Studies on the Improvement in Humidity Resistance of Inorganic and Organic Pigments in "927" Acrylic Lacquer
PERIOD COVERED: November, 1968 ~ July 15, 1969 (Part time)
SUBMITTED BY: J. Jackson
Date Submitted: 7/21/69
APPROVED BY: W. S. STRUVE
Date Released: 7/23/69
ABSTRACT
This report summarizes exploratory studies on improvements of humidity resistance of "Afflair", "Krolor" and quinacridone pigments. Substitutes for basic nickel carbonate (light stabilizing agent for QA pigments)and calcium Staybelite (texture agent) are being evaluated by exterior exposure.
DUP050081468
I. INTRODUCTION
TABLE OF CONTENTS
Page No. X
It. SUMMARY AND CONCLUSIONS
1
III, PATENT STATUS
1
IV, EXPERIMENTAL
A. "Rrolor" Studies
2
B. "Afflair" Studies
3
C. Study on Effects of InorganicExtenders
4
1. A-133-D
4
2. Substitutesfor Basic Nickelous Carbonate 7
3. Studies on Quinacridone Pigments
8
4. Studies of Metallo-organicExtenders
9
5. Studies of Organic Coating Agents
9
6. Studies of Inorganic Extenders
10
V. REFERENCES
1. NB 1815, 1901, 1919K - DSN 69-1
2. Monthly Summaries - JJ - Nov., 1968 - July, 1969
3. K. Batzar, KN-68-3
4. H. Matrick, KN-69-6
5. Unreported work by c. W. Manger (1968-1969 physical Chemical Research Monthly Reports)
Funke, Zorel and Morthy "Interfacial Effects in Solid Paint Films Related to Some Film Properties" Journal of Paint Technology, Vol. 41, #530, p.210,
1969.
DU P050081469
I. INTRODUCTION
The growing importance of humidity resistance testing for auto motive finishes has imposed greater demands on our pigments. Several of our major products were deficient in this characteristic. These include representatives of our QA, CPC, and "Krolor" lines and all of our "Afflair" pigments.
These studies were designed to aid in overcoming this problem and were carried out simultaneously with work by B. J. Godfrey, c. w. Manger, and R. F. White and others.
II. SUMMARY AND CONCLUSIONS
A. "Krolor" products of apparently acceptable humidity resis tance levels are being manufactured utilizing the Emery 3554D/ Igepal CO710 texture treatment in place of calcium Staybelite, coupled with better washing. This results in a high level of humid ity resistance in acrylic systems and acceptable performance in plastics. Alkyd gloss levels are degraded by this operation. (See KO-789, KY-788-D, KY-795-D.)
B. A well-washed, unextended quinacridone maroon, RT-920-D, 59160, has been prepared and submitted to the trade for use in humidity resistant systems (see R.F.White "Monastral" Maroon, RT-920 Check List dated 1/16/69).
C. Cobaltous oxalate extended QA's are on exposure in acrylic systems. This material does not degrade humidity resistance as does basic nickel carbonate.
D. Various metallo organic and inorganic extenders are being studied as potential replacements for calcium Staybelite in QA and CPC pigments.
E. Samples of A-133-D and A-36-D have been submitted to F. and F., Flint, as humidity resistance stabilizers. No reply on these has been received.
F. SOme improvement in "Afflair" humidity resistance has been accomplished by Si02 coatings. This work is receiving further study.
III. PATENT STATUS
A, Patent coverage of the Emery/Igepal C0710 system is probably precluded by public use (R0-789-D) and chrome yellows.
B. The patentability of cobalt oxalate and modified A-133-D for this purpose should be considered.
DUP050081470
2
IV. EXPERIMENTAL STUDIES
A. Code K0-789
Humiditv Resistance Studies on "Krolor" Pigments
Exot.# Treatment
Result
1877-34 Calcium and zinc Staybelite treatments,
Markedly degrade resistance in "927" lacquer.
KY-781-D 1877-51
A. Untreated control) All
>
B. Emery 3554/Igepal) washed
C0710 (low)
) to
C. Emery 3554/Igepal) 6000
C0710 (high)
) ohms/
D. Neofat 10
) cm2
E. Dow-Latex (Styrene)
P. Petroleum sulfon- )
ate (low)
)
<5. Petroleum sulfon- )
ate (high)
)
Control (excellent) WS ws
Vsl ws
Ws SI better Vvs ws
SI ws
Conclusion: Well-washed "Krolor" (without calcium Staybelite treat ment presents no problem of humidity resistance. None of the sur face treatments applied benefitted the humidity resistance proper ties. All treatments were satisfactory for thermal stability and
abrasion resistance in plastics,
KY-781 1877-59 Emery 3554D/Igepal CO710
Treatment plus washing to 4500
ohms/cm2 excel
lent humidity resistance and
abrasion resis tance in poly styrene.
KY-781
1877-60
Further study of Dow-Latex Emulsion DL860 from 68-90% "Krolor" showed this polystyrene treatment
rendered pigment incompatible with "927" lacquer
system.
KY-787
1877-62
Emery Igepal treated slurry ex. plant lot KY-787, 59885 (after SiOa-acid treatment) coagulate with Ala(S04)3 and treat. Wash to 6000 ohms/cm2. Re
sulted in excellent abrasion and humidity re sistance properties (much superior to KY-787-D, TS-91005). This product is presently manufac tured as KY-795-D. (The work on scale-up was
done by R.F.White).
DUP050081471
-3-
KY-781
1877-64
Non-organically treated "Krolor" filtered and washed to 6000 ohms/em shows excellent humidity resistance in "927'' lacquer. Gloss levels are lower than the Emery 3554D/Igepal C0710 treated
counterparts *
Overall Conclusions
in the opinion of the writer/ all "Krolor" products for use in acrylic lacquer should be made with an Emery 3554D/lgepal C0710
treatment coupled with washing to an 6000 ohms/cm2 endpoint (similar to KO-789-D). This treatment is satisfactory for use in plastics
applications.
Products made in this manner are lower in gloss in alkyd systems than calcium staybelite-treated counterparts. Further attempts should
be made to develop a surface treatment that would increase dispersi bility and gloss levels without harmful effects on humidity resis tance.
B* Studies on humidity Resistance of "Afflairs"
"Afflair" pigments evidence very poor humidity resistance
characteristics in "927" acrylic lacquer systems. Simple improvements such as better washing to remove electrolytes do not appreciably benefit this product type as it does "Krolor" or QA pigments. Several attempts have been made to alter this characteristic.
Reference
1815-63,70
Treat NF-123 and NF-133-D with various agents to (a) remove soluble salts, (b) alter basicity and acidity characteristics, (c) make pigment surface hydrophobic. Use of triethanolamine, Na4Pa07, Emery 3554D/Igepal C0710, fatty acids, and petroleum sulfonates were studied. Sodium pyrophosphate treatment showed some
benefit but to a very limited extent.
1815-70
Study of Empol 1040 (a highly polymerised carboxylic acid ex. Emery Industries) showed definite but in
adequate improvement.
1815-71 1919K-2
1919K-11
SiO$ deposition (as per "Krolor" type technique) upon the surface of "Afflair" pigments have shown some im
provement in humidity resistance and gloss levels. These processes are receiving further study.
1919K-13
A study of the effect of sieve size of a given "Afflair "Afflair" (NF-133-D) showed interesting difference in
behavior (i.e., larger particle size, lower gloss) and an unexpected result that humidity resistance
was not effected by particle size.
DUP050081472
-4 -
Reference
SW-00041
Uncalcined "Afflair", stabilized by means of an iron pyrophosphate treatment, shows poor humidity resis tance in "927" lacquer.
C. Studies on the Effects of Inorganic Extenders
The finding by H. Matrick that the addition of ea. 10% A-133-D, SD-00122, via dry blending benefitted the humidity resis
tance Of quinacridone in an "807" acrylic lacquer system is of considerable speculative interest.
Subsequent work by the writer illustrated that this beneficial effect was shown particularly by the standard lot #00122 in "926" lacquer and not by random lots of plant production. A study was undertaken to determine the reasons for this.
Reference
1815-64A-D
Study effect of varying Pe*s/P207~4 ratios. Conclusions Increase in use of Na4P207 resulted in A-133-D of inferior humidity resistance effectiveness
in blends with RT-920-D, 59160 (100% "Monastral" Maroon toner - well washed). Quantities of Na4P20-7 above 190 gr. mol PeS04.Ha0 were detrimental. Good
performance was shown by lab samples A, B, C.
1815-646
Reducing water solubility of product by treatment with Ti0S04 (see KN-54-16,18) was beneficial to humidity resistance. This finding should be studied further.
1815-69
A study of heat development of A-133-D at various Pe+s/p207"4 ratios showed no beneficial effects
resulted.
SW-00064, DSN69-1
This was an attempt to duplicate the excellent results shown by standard lot 00122, Semi-Works and labora tory-washed samples were processed and tested in "927"
acrylic lacquer for humidity resistance effects in blends with RT-920-D. None were fully equivalent to lot 00122.
SW-00072, DSN69-1
A second lot duplicating 1815-64A and differing from
00064 in strike temperature and Pe+3/Pa7 "4 ratio was made. This material, when tested in "927" lacrylic humidity test, closely duplicated standard lot 00122
and reduced the discoloration tendency resulting from
microblistering shown by RT-920-D. This lot, however, is still not fully equivalent to 00122 standard which remains unique. Subsequent tests on a new proposed standard lot manufactured in the plant (92517) showed it to improve RT-920-D but not to the extent of lot 00122. These materials have been placed on exposure in Exp. $er. 69449.
DUP050081473
-5 5 lbs. of SW-00072 were sent to Dr. S. Arora, Flint, Michigan in May, 1969. No report has been returned by F. and F. as of this date. Table 1 summarizes analyses made on various products in an attempt to characterize the cause of these varying performance. The following conclusions may be reachedi 1. Humidity resistance effects do not correlate with the degree of hydration of the A-133-D. 2. A high degree of correlation is shown with sodium ion content. This is probably also related to effectiveness of washing (Na2S04 removal) and to the variable amount of Na4PgC>7 in solid solution (See KN-54-18). 3. Degree of crystallinity of A-133-D had no apparent corre lation.
DUP050081474
T a b le
6
"fr 00 CN CO in 00 00 CO in
,,o *
r-~ crv
rH o 00 O' 00
Oil m CO d*
'O' CO CO CO
CO in CN CO oi oo
00
| VO 00 <n VO CO CO H VO
^,, P0h I
CO
* <*
oi
CO
CO
CO
t CN
rH
CN CN CN CN CN CN CN CN
r in
CO J 'd<
H in rH rH O'- 00
H sn*o''*]1
in o
'd'
oD i-l CN
CO 00
CN VO
VO CO
t" CSI
w ml
fC H
in CM
c\ <n
00 oi C-' CM
- 1 CO CO d* VO vO
in r*
rcHo ir-nH or-Ho 0i--11 HCN orH>
/
m in
in
o]
CN
CN
OI
00
c~*
01
CM
in
^M
01 CO OV r>
t"
w d1 d* in d* d1 d* d* d*
w
H in o in 00
CO vo oi CN 00 rH 01 H
0 ,, <"1 ^ Ph I 01 Oi in
CT1 00 g o " VO
CN CN CN CN CN CN CN CN
m
3 00 vo CM CO t- d- CO
O VO d* iH o VO VO d<
SH 4 o C' rH CN d1 f" d* CO
X)
1H
< Cl rH CO on rH CN 01
,, >i d* CO t" C'- 00 VO s 00 *
rH
OS 0
+>H>1 4g0-) TWe3H0 "PWHa0S
r--1 ooP00P
0wH) 0
&0
uCO
%
T0PO
1 rwi 1
0
Ct-Ol
I
uoCO
*0 Q
dt d1
0 VO VO Q w
rH
CN 1
1 d* d* CN C" CO
Q< CN in in vo VO Cl OI I--1
rH .rH rH o o in 00 o
o oo 00 o o CO 01 o w o rH rH o o in in VO
DUP050081475
-7 -
Studies were made on other ferric phosphates as well as other metallic pyrophosphates.
Ref.
Effectiveness - "927" Lacquer
1815-64E 1815-64F
Peg (Ps Oj q ) a FeP04
Slight worse vs 100% RT-790-D Slight worse vs 100% RT-790-D
1815-65
Mtt2P207.Na4P207xH20 (A-22-D)
Worse VS 100% RT-790-D
1815-68 Ni2Pa0?. Na4P207xH20
Slightly worse vs 100% RT-790-D
2. Substitutes for Basic Nickel Carbonate
Reference
1815-67; 1901-16,17
The finding that basic niche! carbonate (N-947) dry
blended or wet precipitated in presence of-QA's degrades humidity resistance in *'927" lacquer is very serious. This material is added to various QA's to aid in improvement of exterior light stability.
A series of preparations were made from Nicl2 and NiS04 varying the Ni2/co3 ratio and also attempting to vary particle size.
As anticipated, change in the anion did influence
the result with Nicl2 being the better source when
coupled with lower amounts of C03~> Increases in particle size apparently worsened the humidity re sistant characteristics. 10% of 67A (NiCla - low C03*) resulted in only a very slight degradation of
KT-920-D, 59160, versus the marked degradation shown by N-947. This approach could be taken if necessary for maximum light stabilization.
1919K-1
Nickelous phthalate was prepared and tested as a possible substitute for N-947. This material was unsatisfactory.
1919K-3
Ferrous and nickelous ammonium phosphates - unsatis factory in humidity resistance.
1919K-4
Cohaltous ammonium phosphate - uns atis factory in humidity resistance.
102-29 102-32
Cobaltous carbonate is a light stabilizer for QA pigments. Its humidity resistance is similar to
basic nickel carbonate.
DUP050081476
8
1919K-4A
Cobaltous oxalate was found to be a satisfactory material for humidity resistance in "927" lacquer. Its light stabilizing action on QA pigments is being studied in Exp. Ser. 69449.
1919-4B
The corresponding nickelous oxalate was unsatisfactory.
1901-16
Nichelous hydroxide harmed the humidity resistance of QA maroon.
3. Studies on Quinacridone Pigments
The need to eliminate clacium Staybelite from "Monastral" colors to improve humidity resistance is well established. Alter nate treatments are being reexamined using compounds where dura bility data have been previously established, wherever possible.
Two principles are being tested: (a) render surface more hydrophobic, and (b) render surface more polar to improve dispersi
bility in system.
Reference
1910-15
Series 1901-15 utilized approximately 10% of Emery 3554D/lgepal C0610? Neofat 10 (Cio Fatty Acid!? Empol 1014 (C36 polymerized dicarboxylic fatty acid; and Empol 1040 (C54 polymerized tricarboxylic acid as a slurry treatment of "Monastral" Maroon presscake. All treatments were superior to calcium Staybelite in humidity resistance - none enhanced this property, i.e., all were equal to or worse than unextended control (RT-920-D-type).
1901-14
Series 1901-14 was based on this approach, but employed the surfactants in the acid extraction of the dispersion-milled powder. This has given rise to an interesting result with Empol 1040, i.e., the humidity resistance was superior to unextended control. The mechanism of this superiority, i.e., it is due to particle size change, particle charge,
i.e., A1 salt of polymerized acid, effect on vehicle system (acing in manner similar to plasticizer, etc.) should be studied further.
1901-18
"Monastral" Maroon extended with 7 to 22% of the aluminum salt of Empol 1040 showed diminishing benefit
to humidity resistance as the extender was decreased. Rheology seems satisfactory versus RT-920-D, 59160. These products are being placed on exposure.
1901-44,53
Surface treatment of "Monastral" Maroon and Maroon B with "Volan" and Volan L", DuPcnt methacrylate chromic chloride, showed the former made these pigments more humidity resistant. This approach is receiving further study.
DUP050081477
-9-
1901-48
SiOg coating of "Volan"-treated "Mcnastral" Maroon
resulted in products of extremely poor humidity resistance.
4. Studies of Miscellaneous Metallo-Orpanic Type Extenders
Reference
1919K-6
Two forms of the aluminum salt of a petroleum sulfo nate were proposed as possible extenders for use in QA's to improve texture. Aluminum petroleum sulfo nate coagulated with Armac T seems to be satisfactory. Further study via precipitation in the presence of
QA's or CPC's should be undertaken.
1919K-11
An attempt to improve the gloss level and humidity resistance of "Afflair" NF-133-D/ by precipitation
of the aluminum salt of Empol 1040 (polymerized tricarboxylic acid) showed only very slight improve ment. This should be studied further since the humidity resistance level of NF-133-D is extremely
poor.
1919K-15
Precipitation of the 'Al salt of DAXAD-11 showed small but significant improvements on NF-133-D.
5. Studies of Organic Surface Coatings
Reference
1919K-16
Attempts are underway to polymerize polymethyl methacrylate on the surface of "Afflairs". Preliminary results indicate PMM was applied to surface (rendering it hydrophobic). This lead is being currently studied.
6. Miscellaneous Inorcranic Extender Studies
Reference
1815-66
Mn(OH) a is a good light stabilizer for QA pigments. This mater ial was found to be unsatis factory in
humidity resistance.
1901-P-52 (SW-00023)
A-36-D (85 mol % Cr+3/l5 mol T Fe+3 OH3. This highly
durable grey transparent extender showed good humid ity resistance properties. A sample was submitted to F. and F. for evaluation. To date, no reply has been received.
1901-P-53
F-115-D, extremely small, well-washed ferric hydrate, has no effect on humidity resistance in blends with RT-920-D.
DUP050081478
- 10 For purposes of record, work by others has shown harmful effects from admixture of Blanc Fixe (BaS04), A1(0H)3, and aluminum benzoate in this application. Chromic petroleum sulfonate extensions of CPC blue or green (6-446, 0-798) show excellent humidity resistance in TEA 3 lacquer. The base material, unextended, was found to degrade the humidity resistance of "927" type lacquer.
DUP050081479
6 U
ss
Ck
c/)
15 **>S32
g 555
s
* V
3 H
JiHt
Q) r <%<P
O _.. a
&i
> 3 ^ S`3
W.u<u
I I$
DUP050081480