CC: W. D. Cobb-PID-Wilmington D. P. Rapp-PID-Wilmington W. E. Robinson-PID-Wilmington L. L. Patin-PP&R-Sabine J. W. Martin-PP&R-Sabine G. R. Sigler-PP&R-Sabine J. R. Breitenstein-PP&R-Sabine J. L. Gossett-ESD-GRO-Beaumont R. W. Ross-c/o Sabine Const. E. S. Mazanek-c/o Sabine Const. J. W. Atcheson-Construction C. A. Seibert-Des.ign H. E. Huckins-Design
~>II. Ii: Bowman-Design A. A. Gruber-Design W. D. Muto-Design IC 32-Process Design
v,L,, ft], I (4 f -- 11 O
-*PXP
WR-437169 - SABINE - SPECIAL PROBLEMS ASSISTANCE WET INSULATION AND STAINLESS STEEL
Confirming the attacked ESD recommendations, current Sabine PID projects should be started up without removing wet insulation on stainless steel pipe and equipment. As indicated, wet insulation which was in place but not covered by jackets during the strike should be replaced. Also, after start-up, the insulation should be checked to be sure that it has dried and is effective.
DESIGN DIVISION Polymer Intermediates Section
G. E. Buchwald Senior Process Engineer
GEB:jj
attachment
DUP 0827162
* A
May 3, 1976
cc:
A, A. Gruber - Design J . L. Gossett - ESD,GRO - Beaumont T. w. Gibbs G. E. Lang F. T. Wyman IC 13 - Materials Engineering
TO: FROM:
G. S. BUCIOTALD^^ DESIGN DIVISION
W. E. ELLIS j()(.
ENGG. SERVICE DIVISION
POLYMER INTERMEDIATES DEPARTMENT - SABINE RIVER WORKS MATERIALS ENGINEERING WET INHIBITED CALCIUM SILICATE INSULATION IN CONTACT WITH
300 SERIES STAINLESS STEEL
A review by several members of the ESD Materials Engineering Group of
chloride stress-corrosion cracking of stainless steel under wet
inhibited calcium silicate insulation suggests that we can start up a plant with the wet insulation .and have reasonable assurance that no
failures will occur. Stainless steel pipelines and equipment which
Will operate below 40C do not have sufficient
f-n
chlorides to a level where they will h* Virt-rm-Fni
oanco <->. i
stress-corrosion cracking. Stainless steel equipment operating above 4Q^C does have this ability but can concentrate only those chlorides
available in tne lns'ul&tlCTr: to cause failure of the stainless steel equipment operating above 40C, in the presence of silicate inhibitor, we believe that it is necessary to add chloride-bearing water by con tinuous wetting of the insulation by rain (may contain 30 to 50 ppm
chloride) or by washing the equipment or the adjacent floor areas with a brackish water (high chlorides 1,500 to 10,000 ppm). Time to cause
cracking under these conditions is related to the temperature and the chloride content of the water being added to the insulation.
Based on this, we believe that even though some insulation may have become wet in the construction of these plants, they can be started up without removing the wet insulation. However, we do recommend that any of the insulation which was in place but not covered by aluminum jackets during strike should be replaced. After start-up, the insulation should be chocked to be sure that it has dried and is effective.
Many tests have been conducted at the Engineering Test Center which support our thoughts on this subject. Some of these test results and information are included below.
Standard Wick Test Using Stainless Steel U-Bends
Fifty U-bend specimens were exposed to the standard wick test and only one failure occurred when new stock material was used in the test. We have had no failures from insulation supplied by Papco. One specimen
DUP 0827163
2- May 3/ 1976 G . E. Buchwald
cracked x?hen it was tested with a stock sample supplied by Keane. Several wet insulation specimens were gathered from various pieces of pipe and equipment and used in the wick test. Of 35 U-bend specimens tested in contact with wet insulation, several showed pits and one group of five specimens showed three cracked specimens. This particular test was run from wet insulation obtained from a pipe, and sections generally are small. It is questionable whether we had a standard block of insula tion from this pipe? therefore, abnormal wicking may have occurred.
Chloride and Sodium Silicate Analyses The Engineering Test Center has had several samples submitted for a soluble chloride and soluble silicate analysis. In some cases they were dry samples from stock and in others they were wet samples from the equipment. In all cases, the soluble sodium silicate ranged from 8,000 to 14,000 ppm. The chloride content of the dry specimens from stock showed chlorides less than 400 ppm. The wet samples taken from pipe or equipment showed the chloride to range between 600 and 8G0 ppm. In all cases the pH of the insulation was 9.7 or higher. The chemical analysis of the soluble silicates indicates they are present in wet insulation is sufficient quantities to prevent cracking in the wick test. Military Specification We know that all of the insulating materials we have used on stainless steel equipment will pass the chloride stress-corrosion cracking test required by the Government in their Military Specification, 124244. This military specification describes a chemical analysis to determine sili cate to chloride levels present and their ratios. In addition, a wick test is required which will not chloride stress-corrosion crack a stain less steel U-bend when distilled water is used as the wetting solution.