Document jgx7g2gD3Yaa72deX5My5qgMN

V EjrSl . DC PO\T DE \EMOCRS ^ COMPANY <l\C.) THE ROCKBESTCS PRODUCTS COR?. New Haven 4, Conn. Attention: Mr. C. R. Berlepsch ._ . / 5-'.\ Dear Mr. Berlepsch: The wire sample which you submitted at our February l8th meeting has been Inspected and the following observations made: SAMPLE: TL 203VB 1 "Mylar1' Tape - Failed approximately 2 months, 1.0 K.V. OUTER GLASS 3RAID - WHITE WITH SLACK TRACER Outside surface discolored to a light tan over area under test foil. Ko discoloration evident or. under side of braid which was against the asbestos sleeve. No persis tent odor present. IMPREGNATED ASBESTOS SLEEVE Normal grey white color changed to light tan along entire length of test area. The tan color is present throughout the volume of asbestos although slightly darker spots appear on the surface in contact with the glass braid. Strong acrid smell is definitely produced by the discolored asbestos. Outside the test area this material is odor less in the small quantities tested. The discolored as bestos appears to be somewhat drier than that outside the test area. 1 MIL "MYLAR" A - 1/2 INCH TAPE - BETWEEN CONDUCTOR AND IMPREGNATED aSSSStos Over entire test area "Mylar" film was heavily populated with small oblong holes occurring roughly in lines ex tending along the machine direction of the tape and hav ing ragged edges visible under magnification. The as bestos adhered to the "Mylar" in spots along test area only. Simple visual inspection and handling indicate no em brittlement cf the small sample tested. A slight opacity and the physical shape to which the tape tends to re vert after being removed from the conductor are indicative SETT >'. Th NOS * C BE' f E 9 : RBB 01380 THE &GCEBEST03 PRODUCTS COR?. FEBKUAKX 25, 195* of heat treatment during some portion of the manufactur ing prodea* following application of film to the con ductor. Discolored over entire length of test area. A green compound appears in relatively large amounts between the outside strands of wire when viewed under magnification. Outside test area tnis wire has a bright finish with no evidence of corrosion. This information will no doubt be similar to your own observations of these samples. A chemical reaction has taJcen place resulting in the degradation of the asbestos impregnant. The number of holes in the "Mylar" cape irwic&xe a strong possibility that at least a few openings were sresent for sometime before failure occurred. As stated in the masting, we are vitally interested in this prob lem and do not feel that the performance noted, even under the severity of the pOOO volt test, is typical cf "Mylar" polyester film as regards a.C. voltage endurance. Upon receipt cf the sample wire from Rocttbestoa, we plan to init iate tests at this Isaor&sory wr.lch will undoubtedly be effected by the results or your evaluation rf the '`Mylar**-glass braid or a "Mylar'-unimpregnaced asiercca-gi&aa traid insulation system, and on the first results of your existing nMylar"-Cellulose Acetate butyrate-impregnated asce&toa-glass oraid system. It will also be very helpful for us to zr.ow the exact chemical composition of the lapregrunt ised m the asbestos sleeve as well as a brief des cription of the manufacturing process for the TL 203VB wire. We would lijce tc held a second meeting with members cf your concern after we have had time to review our findings and determine a definite course of action. your cooperation in tne matter is appre ciated, and do net hesitate to contact us regarding further develop ments in your use of "Jtylar" polyester film. Yours very truly. DLOremh D7 L. Ormond ^ SALES DEVELOPMENT AND TECHNICAL SERVICE LABORATORY RBB 01381