Document jgoyB1EzDzNj2mkp1MB2eB0xQ
- - '32-
> '- T-r -' ^ -- _ - -
-r-3&**Z7h-r
. i if:r:::-""- s^'
IKXBAETO CHWICA1 COMPARE
* . .
_ aAUSM'S MAIOAL "
'*
AROCLOR
-
-*5 &S.V~* Jggj' %
^r -
r
y\ r--. *
DESCRIPTION AND PROPERTIES
* .*: >:* \.\
The Aroolors are aserles of chlorinated hydrocarbons based on
biphenyl and terphenyl. They are. not pure compounds bat are
mixtures of closely related chlorine substitution produets nan-
ufactured essentially to a set of specifications based os physical
properties rather than chemical composition.
_
.r.r
The approximate chlorine content is indicated by the last.two
figures of the Aroclor number. The chemical composition closely
approaches the average for the Indicated chioro-derivatives as
follows,but should not be represented as slsqple chemical ecsqpo- ..
sltlons according to the formula shownj
-
""
Approximate Equivalent Chemical Cosgound
. *.* f*** i.
- -
Pl219*f
Monochloroblphenyl
; 123d . ! 124*
Dlchloroblphenyl Trichioroblphenyl
' 1249
Tetrachloroblphenyl
1254 - - Pentachl oroblphenyl
120 _ Hexachloroblphenyl
126? . Heptachloroblphenyl
1268
Wonachlorobiphenyl
1271 ; Decachloroblphenyl
5460
Ronachloroterphenyl
43?2? - -:w.
*r ... v.
SF ' S----- ^ --
Va?-.
Reference should be made to technical bulletin P-115 for tables"
and graphs of .physical properties. This manual contains only that'- "
Information which is not designed for general public distribution
or has been made more recently available than permitted incorpora- ``-~
tion in the printed.bulletin. .
'zk:-- T-T^;
- sr* ,
J.i
-- --7
..
" t '
.
'ear^T*
' ' . '.fcfcl ' * --------v]
* -rn - j.1
The following Aroclore list In eonmerclal production (but availableX j
have been .proposed.-> -sk&k1
Pined Chlorine... Color (toviboridT Pour Point Softening, fg&k-
,47.9*^=,. 54.835^311
" 6.0T
20.a *!^f -
3~
TOWOLDMONOOOI578
MONSANTO CHEMICAL COMPANY
10-1-44
Aroclor No. Viscosity 98.9C (210P)
5448
2151
395.0*** *** -
Plash Point Burn Point
250C 400C
m
Chlorides Acidity - mg. KOH/g.
None 0.008
None 0.004
Evaporation
-
Resistivity Ageing Dielectric Constant
SD3
0.006
-4.65
0.007
-- . 4.17 J
DIelertri
ELECTRICAL-PROPERTIES
4^ /> Aroclor Aroclor Aroclor Aroclor
'
1248
1254 _ 1260
5442
Constant 9 l'fco5^
4.63 4.15-4.35 3.6-3.8 4.92
1
Resistivity <9 100^ Dielectric Strength
500x10^ Above Above JRjOxlO* 500x10*
3^KV Min.
1469x109
Power Factor (100C 1000 kc) Less than 0.1*
Less than 0.1J6
* IRS Method H-3955871 ** Resistivity 9 100 under 500 Volts DC *** ASTM D-177-11
Refractive Index
Range
Aroclor 1270
"-
Aroclor 1271
Tetradecachlorometaterphenyl
Tetradecachloroparaterphenyl
1.691-1.74
1.691-1.74 1.712-1.718 1.691-1.74-
Heat of Vaporization
Aroclor 1260 Aroclor 1262 Aroclor 1169
3 bid. pressure) * 760 mm. pressure)
0.151 atm. 9 350C> 0.079 *ta. 325CJ
Midpoint
1.712 1.712
1.712
B.I.P./lb.
104 72.4 69.2 70.6
1
GBRN002015
TOWOLDMONOOOI579
MOR3ANTO CHEMICAL COMPANY
10-1-44
SOLUBILITY
Solvent
Aroclor 1268
Cold
Hot
Acetone
Alcohol, Formula 3-A
Amyl Acetate
Amyl Alcohol
Benzene
Butyl Acetate
N. Butyl Alcohol
Carbltol
Cai^onDi^uUiae
CellosoIvT
Chloroform
D1 Butyl Phthalate
Ether
Ethyl Acetate
Ethyl Lactate
Ethylene Dichloride
4o Formaldehyde
Furfural
High Test Gasoline
Glycerin
Kerosene
Linseed Oil
Methyl Acetate
Mineral Spirits
Paraffin
Phenol 90#
Pine Oil
Pyridine
Toluene
Tri Cresyl Phosphate
Tung Oil
Turpentine
Xylene
dJL^M.
a* S PS
s
s I I
s s
s
PS I s I PS
I PS I PS
s*
PS s s
s s
A.
I I.
s
3
as
PS
s s s PS s
s
I PS
I
s
3 PS
s s
3
s
s 3
yiS.*or*JT>*C
I Insoluble PS a Partially Soluble
3 a Soluble
Solvent
Gms. Aroclor 1270 per 100 cc.Solvent
Approx. Temp, at which soln.complete
Furfural
Furfural
...
Secondary Amyl Acetate "
Secondary Amyl Alcohols
Carbitol
.
Heavy White Mineral Oil
2.0 . 4.0
4.0 4.0
4.0 4.0
105-110C 120-125C 110-115C Not completely soluble at boll Above 125C-
110-115fe
' ojsicsr-
..-jjgflfci-**" -- t BBRN0020 16*
TOWOLDMONOOOI580
M0SSANT0 CHEMICAL COKPAHY '
- 10-1-44
STABILITY
Toward Heat
Aroclor 1248 was heated to 650P In stainless steel autoclave with the resulting changes Indicated In the following tabulation:
Time of' Heating (Hours?
Temper . ature _______
Acidity
mg.KaOH/gm. Aroclor 1248
Original Sample Autoclave #1 Autoclave #2
Autoclave #3
0--
331 343C. 650F. 500 343C. 650F. 669 343C. 650OF.
.0021
.0392 .0809 .0800
These results are interpreted as indicating very^excellent stabll
lty for Arodors under the conditions of test.
.*
Toward Oxidation
When Aroclor 1254 is-heated for 50 or 60 days at 150C in the presence of oxygen and copper, there Is likely to be seme attack on the copper. Examination of Aroclor 1254 after that period of time will usually show the presence of soluble copper. This also
occurs with mineral oil and other insulat.ng liquids.
In general, even after severe oxidation conditions no evidence of chlorine splitting from the parent hydrocarbon has.been found.
Toward Acids .
Arcclors 1242 and 1254 were stirred with an equal volume- of con
centrated Sulfuric Acid (98%), dilute Sulfuric Acid (10%), Hitric
Acid (70%), and dilute Hitric Acid (5%). at room temperature (25C)
for 150-250 hours. The Aroclor was then washed until neutral, de
hydrated with Sodium Sulfate, then analyzed in comparison with a
control sample for the various properties which are regularly con
sidered, without causing these properties to depart from specifica
tion limits. ..
..........
'. .
Aroclor 1262 was treated for 160 hours suspended in the same acids
as above at 50 to 55C. The concentrated Hltrie Acid caused an
increase in color, otherwise no significant change in characteris
tics .
.
.. . : .
The acid layer from the treatment of Aroclor 1254 was concentrated
Sulfuric Acid at room temperature for 150 hours and was tested for
chloride content. The quantity of HC1 found was so small that it
was not possible by ordinary methods to obtain a quantitative fig
ure. Thus it appears that practically noj4ydrogen~chloride, is. ~
evolved under these conditions. `
..g-. .
-N. *.-
. . ---- * . T *
'"vh.rj&St 'Ta *^*"i?^**- ! /Jn tT\*rsv. *--' *
GBRN002017 .:.
TOWOLDMONOOOI581
conosioir
Additional corrosion data not included in bulletin F-11S (FI 4-43-B) la aa fc--------- * -
Monel
342C
Doe Metal
. 150C "
. Yellow Bras a ;325C
-
11 alloy 17ST 120QC
A1 alloy 525H 120C
A1 alloy 53d* 120oc
360 hrs.
.000
.. 40 days . *001 .:
'.
2,960 hrs. *. . >003, ...
in steel boab V
. . '
21
`100035*
'
21 -
> -- .00035*
21
.00038* ~
.
*The weight loss occurred In the first seven days of '
the teat, negligible loss was encountered In the
' laet 14 days.
' ;~
1.
The vapor condenser and* the product receiver of the plant distills-
tlon unit for producing Aroclor 1254 is construeted of Monel and no:-
fallure in the system nor any noticeable reaction between the Aro-
clor and the Monel baa been discovered after three years of opera
tion.
...
_ .: .
.-
SQLPBUiITY OF WATER IN ABOCLOB 1242
The water content of a sample of Aroclor 1242 saturated with water
at approximately 30C vaa determined,using the Karl Fischer reagent,
to be about 0.0o*
--..............
: .............
............
Aroclor 1242, as regularly produced, contains by the same test less
than O.OOljt water,
.r--
.
v.
' ''
SURFACl TENSIOW
' /`
The surface tension of Aroclor 1254 Is as follows:
TOWOLDMONOOOI582
-"S' 'ir-'r. NOABTO CBBmCAL CGKPAJBt, /?*-
jfe-4*
? Acute yellow atrophy of the liver la which the liver
cell! show evening, hypergranulation, hyaline inclu-
elone end vacuolatlon a a result of extensive. expo
. sure over long periods of time. - -
-.
These symptoms may also result from exposure to other chlorinated
hydrocarbons of canoeroe, such ae j carbon tetrachloride, diehlor-
ethylene, trlchlor ethylene, chlorinated naphthalene (Bblov&x).
The best known (at present) measure of the degree of toxicity of
the Aroclore Is presented belovs , ;
... .
.
' Permissible Limits (in ag./cu.m.) of Concentration in Air of Work Rooms: (journal or Industrial Hygiene A Toxicology 21: 1537" 19397
Tested on Rats by Inhalation
"
Chlorine Permissible
- -
Content
Limit
,1____ mjg./cu.m.
Aroclor 1268
"" 66 - 10.0
Aroclor 4465 Aroclor 5460
65 '
0.5
60 0.5
Aroclor 1254
5% 0.5
Trichlornaphthalene plus trace Tetrachlor-
naphthalene Tetra and Pentachlornaphthalenee
49.? 56.4
10.0 * 1.0 *
Penta and Hexachlornaphthalenes
' 62.6 .. , 0.5
Tetra and Pentachlornaphthalenee plus
. *. . ...
Refined Chlorinated Diphenyl
4>.5
- 0.5*
90$ Penta and Hexachlornaphthalenes / 10
Aroclor 4465
' 63.0
/ 0.5 *
Chlorinated Diphenyl Oxide - -
54.0
- 0.5
Chlorinated Diphenyl Oxide
'
Hexachlor Diphenyl Oxide / 5% Trlchlor-
57.0
0.5
.naphthalene
<
. '50-55
0.5
Hexachlornaphthalene and Crude Chlorinated
Diphenyl
......- ..... --
..
--- - __ --
:
a.s
Special Chlorinated naphthalene... . . .. . * 50-5.6 -.
.-5
Tested also by feeding.'
Summary of Gross feeding Hxperlaenta
Of the various material^ fed ~rats~Am large dosee, TWcbioroaphthalene
-: *
plus traces of Tetrachloroaphthalenervae quite Innocuous . Tetra .
'
and Fentachlomaphthalene showed definite- A&vwr damage :-ur Penta and?
-
Hexachlornaphthalenes caused a similar grade' of Injury* The addi-.
-
tlon of chlorinated diphenyl to Teat* and Bexaehlornaphthatenee / '-
increased the toxicity. Chlorineted Diphenyl alon*. produced JSver r-rt.
lesions but in the dosage used vaa less effective; thin to^h mlked' Jl
vlth highly chlorinated naphthalenes. Zh nO ptXtT dl^^g'tFdmpouhd# ~
,awM^.v^'riei r.r ,-mine&nr.saeB***--
GBRN002019
TOWOLDMONOOOI583
used produce abuts yellow atrophy hut the lealone observed Indi
cate this night be poaalble If one found a doeage which could act
for the proper period of tine..
. _v r-
-,V >-"ii
Feeding Precise Poaea by Stomach Tube:. The compounds employed vere . ...,,
auapended m gun acacia, in figuring the doeage the total anount '
a man of 50 kg. could Inhale la an 8-hour day, assuming on air coo-*
centratlan of 20 na. per cu.m., was flret calculated and reduced.
'>
to nllllgraas per kilogram. The rate and rabbits received this ~ .
..
dose each day. The compounds used were those employed Id the gross . '
feeding experiments and the results vere essentially similar though
the lesions vere less severe.
. . - -................ ........
Subcutaneous InJec11 ons* The same gum acacia suspensions vere ln-
jeoted subcutaneously Into rats and rabbits, the doeage being cal
culated on the basis of % mgm. per cu.m, of air. Again similar
results vere obtained. Tn all such experiments there mist of nec- "
esslty be differences In the degree of effect but Invariably the
liver was the sole organ.affected' and the lesions vere those already
described many times.
'
r
>it-
* : '
- ._-*.---
. ;
'5:. -
~-^ 4
Reccnmendationa for Industrial Practice: unless there is a very
/
good reason for using' the hot method oT impregnation, all new Intallatlons should use the cold or solvent method of Impregnation
vlth chlorinated naphthalenes and diphenyls. Where the hot method Is nov being used it should be changed over to cold. If possible, or surrounded vlth every knovn proteotlve measure. . . ...
.
General hygienic measures should be followed, but in no case should
these be allowed to supersede engineering control of the primary
source of the exposure, the operations In the plant.
_
The following hygienic measures may be considered good practice where these compound*, are handled:
(a) Two locker* for edch worker exposed to chlorinated waxes (one.for voicing and one ror street clothes).
...
______...................................................................................... . .... . .. ..
...................................................
(b) * All vorfc clothe* above the underwear should, be. pro- ' ' `
_-
wideb and.laundered at least 'twice a week, by the - ^ -
-- - -*'< :
ianagemenf7;T-jt.;-
....* %
.
r(c). Tbs' workers ^h<ail$change to clean underwear at tha ; \'Tf-'. ead of each shift before getting lnt his street clothes. :
: (d)
_V -
Supervised cleaning: fl). At noon the worlrcra aikMld^-^sx
remove outer clothing and sorub hand* and face ,under -- . supervislon; f2)^'at tbe eal of' the shift thej sho*^^ '^
her required t*t.JajkfL <r. supervised shower^forai:changing back
:'7 VcS -x-.v
TOWOLDMONOOOI584
-v-' * '.......................................................
` m&Amo cmMicAir ccKPAinr
c-: kr :
- . `
; i-
*
. *v J `
(e) Protective skin creams or protaqtivs clothing should be -
provided by the management ah the discretion of the fore-
nan, mures, medical, or plant superintendent*
.
.
(f) All departments handling chlorinated synthetic waxes
should be thoroughly cleaned according to a prearranged
schedule. This should Include the.removal of all depoeite of waxy aaterlal from the machines. floors and surrounding objects. Yorkers doing the cleaning should be provided with protective clothing and supplied air or - organic vapor masks where exhaust ventilation is inade quate or not possible.
The foremen of all departments where this material is handled
should be apprised of the toxic nature of the material and in
structed in safe handling procedures. These men should make It *
their duty to check up on the workers in their departments and
instruct them in safe practice.
.'
Pre-employment and periodic physical examinations should be made
of all exposed workers. These should include the taking of a full
clinical history, with special emphasis on gastro-lntestlnal dis
turbances and dermatitis. In addition, the skin should be care
fully examined periodically and the more reliable liver function
tests performed. Gastro-lntestlnal complaints developing in a '
worker at any time should be a signal .for an Immediate medical
check-up. A history of liver disease, jaundice, or antleyphllltic
treatment should automatically exclude a worker frcsi jobs involv
ing a possible toxic exposure. Pregnant women should not be em
ployed where there is a possible exposure to the synthetic chlor
inated waxes.
. ... .
.
Engineering control of plant operations oannot be over-emphasized
but specific reeconendatlons are not applicable to all. cases. It
would be wise for a plant using this class of materials to check
their control measures with the state Industrial hygiene agency, ,
the Insurance carrier and some competent consultant before occu- [
patlonal disease occurs-- .......................................- - ... -
--1
" "X-"a* - . ?. * *. *c APPLICATIONS OP ABOCLOBS
-* * *
7. . -- -
A&HBSIYES
..
Adhesives of good electrical characteristics can be prepared con taining Aroclors. The following, are typical examples* .
TV".
*v
Typical Values
#103 Aroclor 4465 (Code 3140-0144) (XY> Paraffin 50.8oC , ~^ r -
. Mineral Oil (ExttarBeavy Vhite) * Barytes - Kepham'rli #2 ' :
' >
.zszb&IUM: v- r 50.0* -Tv.
GBRND02021 sfa.-se'*
TOWOLDMONOOOI585
- r" *>'
vTSSe-.-
NOMABTO CSM1CAI* COKPAJW
r: r
,
c Typical Talues
#103B Aroclor 2565 (B.F. 77.5^5) (Code 3140-0114)
(XB) Paraffin 50.8C
'
. Mineral Oil (Xxtre Beavy White - Sonneborn'e)
Barytes - Mephsm'e $2
'
46.506
1.17 a.3> 50.00
#131 B-ll 65B
Aroclor 4465 (Code 3140-0144)
Sster Cum - BBC #12021X0 Pale
Paraffin 50.8C
Barytes - Mepham'S #2.
..
16.1& 14.3* - >55 65.00
#135
Aroclor 4465 (Code 3140-0144)
'
Rater GUm' - BERG #1202XXO Pale
Mineral Oil (Bxtra Heavy White - Sonneborn'e)
Barytes - Mepham'S #2
20.70# 18.45
5.85 55.00
#H Aroclor 4465 (Code 3140-0144)
50B Mineral Oil (Rxtra Heavy White - Sonneborn's)
Barytes - Mepham'S #2
..
46.0#
4.0 ` 50.0
#"Mff Aroclor 4465
; 89.5# '
Mineral Oil (Rxtra Heavy White - Sonneborn'e) .10.5 .
#"H" Aroclor 4465 Mineral Oil (Extra Heavy White - Sonneborn's) Silica (Schults, Champlain ft Blbbo)
58.2# 6.8
35.0
For the preparation of thermo-plasti3 adhesives Purdue University
found that the harder Aroelors are better than anything else dis
covered to date, primarily because of their high compatibility
with other resins and their thermo-slability.
.
. .
.
-
^
.
ELB'C T HICAL
Dielectrics and Electrical Insulators
-. ' ,, .
The Aroelors have excellent dieleotrie properties, that is, low
dielectrio constant and resistivity and low power factor. Aro-
clor 1242 lias, the highest dielectric constant of the whole series
which we are manufacturing commercially, while higher chlorine
Aroclorp have hlgheg,wU_tgjtjv
.. -r;~ .
The Aroclora'have f^ad xieefulnesa ds a dielectric im'condensers
and aa a dielectric and cooling medium in transformers, and a number of miscellaneous similar uses where the characteristics
above named'are of importance. -- ^ iv< rvi"-*?.TrsswKr
-T
'
iiss**
AROCLORS AS SATURAHTS
Saturation may be defined as that operation bywMch liquids or - . -
gases are caused to penetrats relatively porous materials.., The _-Vw
penetrating medium'is knowhaatheseturant and It generally in.
-
TOWOLDMONOOOI586
NOIBACTO CHEMICAL COMPACT
;-T: ie-i-44
the liquid state. Saturation may be assisted or accelerated by .
me axis of increased temperature and pressure or fey the use. of a
vacuum.
: .
. :.. - T'
:.Jz '* '' . '
Various classes of products are saturated for the purpose of giv-
lug them a vide variety of properties. Some of the properties
attained by saturation are: vater and flame resistance$ resistance
to chemicals; abrasion; moisture; light and weather changes; in
creased strength; and increased weight.
... .
t. -
Among the articles that are treated to obtain some one or all of
the above mentioned properties are Included the various fibres and
fabrics: animal; vegetable and mineral; voods, both hard and soft;
ceramics vare and cement; and certain kinds of electrical appara
tus, such as carbon resistors. '
' '..........'
_.
The saturants*, or, as they are sometimes called, the Impregnante,
are usually made up of vaxes, oils, resins, or vater solutions of
certain inorganic salts.
, . ~..m . -
' Applications
At present the saturating applications that are of chief Interest are insulated wire, low voltage cable commonly called network cable, and carbon resistor fields. These proposed uses sre des cribed more fully under the separate headings vhlch follow.
network Cable
- -
'
r 7
Attempts are being made to develop a use for Aroclor as- a saturant for secondary network or Ipv voltage cable. . Cable of this kind Is used In electrical network distribution systems. Generally, It
consists of the copper conductor or conductors, the paper insula tion, and the lead sheath. The paper is saturated with an oil*
usually a good grade of oil such as the General Slectrlo Company's
Trans11 Oil. This form-of construction is objectionable because under the conditions Imposed by s short circuit, combustible gases are generated vhlch flow through the conduits to the manholes, at
vhlch point they may form explosive mixtures vttb the-sir and. In turn, cause explosions In, the manholes. Both the paper and the -oil
are sources of Combustible gases,'. It It therefore desirable to " replace them the paper with am-inert form of Insulation, If possible, and the olP with a non-inflammable saturant sueh as Aro
clor. Thus far, Aroclor 125b appears 'to meat , the requirements of .
this Use, .
, _'
__ ' ' : .' T
~
,v KjyjgSggiSyfp' ~
-
The more' Important cable manufacturers In tbs country are already
at work on the development of a flame resistant^ cable and also one
In
vhlch
the
ex-plosion
h' az-a-- r d-
will --be.
l* e ssenre-dtro- r~
.
emlim4*in*tat ed.;.^-
' ~=
*" " - ; * n.---t.
jW*
JmSSj BBRND02D23*
TOWOLDMONOOOI587
Carbon Resistors
. J.. .
,,
MOXSAJTFO CHEMICAL COMPAHT .
''
.
io-i-44
* 4. . .
.-
Carbon resistors are small molded rods of a mixture of carbon black and sand vlth a resinous binder. They are porous and their elec
trical resistance If seriously affected, by the entrance of moisture.
To prevent moisture getting Into tbs units they are usually Impreg nated vlth 'acane, material to fill up the voids and to coat the sur
face of the resistor. A max is generally used for this purpose and
serves very veil as far as moisture-proofing Is concerned. How ever, after completion, the resistor must be lacquered for ldenti-
flcation. Lacquer does not adhere veil to the waxed surfaces.
Aroclor 4465 Moisture-proofing Compounds give moisture proofness .
(Hisnldlty test) equal to that of vax and. In addition, give a.sur-
face to vhlch lacquer vill adhere.
.,
.,
The Aroclor Compound la non-crystalline and therefore does not have
a definite melting point and does not become extremely fluid at the
melting point of most vaxes that are used In this application, but
It gradually softens under increased temperature. .
.
In extensive tests to find the most effective medium for Impregna
ting radio resistors to stabilise the eleotrloal resistivity under
exaggerated and extreme humidity tests, Aroclor 5^0 gave by far
the best results vhen compared vith Santovax and various petroleum
vaxes and compounds.
.-
This excellent Aroclor success vas accomplished by grinding off or
sanding the surface of the carbon resistor prior to Impregnating, thus exposing the inner pores of the resistor, permitting excellent penetration. Penetration has alvays been a problem In the Impreg nation of resistors vlth resinous materials suoh as Aroclor.
Cable Insulation
Electrical conductors'and cables Insulated with asbestos are fre- ~
quently lacking In vaterproofness. - Impregnation vlth vax composi
tions gives an Insulating medium resistant to atmospheric moisture ,
and -sometime* even to laserslon In water for- a short time* but. . ... ..
hitherto ns-ocnpoeitloo having tbs required characteristics of
.
heat resistance and flameproofnets has given sufficient water re -
sist&nce to.withstand lasers ion for prolonged periods-
-
.
An Improved method of Impregnating'sitesto# is described In U. 3.
Patent 2,162,953, assigned to Rockbestos- Products Corporation,-
vhlch depends on the usq. of a phenolle resin in conjunction, with ,
a chlorinated diphenyl. . Jfc, has already bee& proposed to use each
of these substances ssparetelj^f6a'n
purpose
alone _
the first lacks flaaproofhes and the^^pefCMa^ ^alltano^ioJwater."
TOWOLDMONOOOI588
1.
v' ! ~ *
*>- %
. T-- ` '
. \ - * *r-
. >-....
r MOBAKTO CHEMICAL COMPART
: - `"10-1-44
The phenolle resin used for this purpose should be thermoplastic,
solid and rather brittle at ordinary temperatures, with a floe '
point of 105C. Bakellte ZR 84JO is suggested as a suitable type.
The best chlorinated diphenyl for this process is stated to be one
having a viscosity of 96 sec. Seybolt at 100C, and, of course. It
must mix readily vith the phenolle resin. One containing about '
62 per cent chlorine is said to be satisfactory, for example, Aro-
clor 1262.
.
The tvo ingredients are mixed in equal parts by weight at l6oC, preferably vith the addition of 5 per cent by weight of a plastielzer sueh as Trloresyl Rxosphate. The resulting mixture is stable and can be stored.
In manufacturing the cable the individual conductors are Insulated,
twisted and covered with the layers of impregnated asbestos and varnished cambric (or the like) in the manner well understood in the art. A layer of loosely felted dry asbestos of suitable thick ness is then applied around the thus assembled cable, and a dry asbestos braid is applied over the felted layer of asbestos. The
so-covered cable is then passed through the impregnating compound (mixture of resinous phenolic condensation product and chlorinated diphenyl) while maintaining the compound at a temperature of' about
c 155C. The time required to impregnate the layer of felted asbes tos and asbestos braid will depend on the thickness of the layer.
As the cable emerges from the heated hath of impregnating, compound, .
it is passed through suitable snubbing devices to remove the excess compound frcra its outer surface.
In order to prevent migration of the outer surface compound when
the finished wire or cable is subjected to high temperatures is
service, it has bees found advantageous in same Instances to ap
ply to the Impregnated layer of asbestos a second coat of the
impregnating compound to which has been added about 15 to 20% of
ground mica or other finely divided inert solid material. The
impregnating compound on- the outer surface of the impregnated
asbestos then contalne dispersed finely divided particles of the
inert solid material which act to thicken the compound and render
it less susceptible to flow. The admixture of mica or the like
is not required or desirable in the compound used to impregnate .
the asbestos layer, since the asbestos fibres themselves satisfac
torily perform the function of retaining the compound within the
mass by capillary attraction. .........
... . .
The insulated conductor or cable of the invention* possesses ail'
the necessary characteristics of beat resistance, flameproofness,
- v-r-
pliability, dielectric strength and resistance to water* The
.
outer insulating layer of. asbestos impregnated, with a mixture of
..
resinous phenolic condensation-product and Chlorinated dlgbenyl
.. D. :,
(
is substantially waterproof, eTen when submerged In water for ex-..
;
tended periods of time or subjected to hydrostable pressure as * ' _ ..
high as 25 pounds per Square hoh- Zjx'9sneral'r ttte use of asbestos^ :
V-rA-JV 4S.* *
'-irar- `7
GBRN002025
TOWOLDMONOOOI589
* .'V-. - .
WUX-H
- ..
WMJUBO CHEMICAL CQKPAJflf -"v "... vV\\ I'-: ">.
at an electrical insulating material bat heretofore been Halted
ta locations there high temperatures or the hasard of inflammable material made the use of ordinary forma of insulation (such a . . rusher, varnished cambric, paper, eto.) undesirable or prohibitive. It till, therefore, be evident that the invention widely extends ,
tha usefulness of asbestos insulated vires and cables, rw . ~v.
~' '
Condensers
... .
A rapidly growing use of Aroclor la in the manufacture of tha small
condensers employed in fluorescent lighting fixtures for offices,
business houses and factories. ,
...
: . _... ___ ...
ABOCLOR EMULSION FORMULA .
:' . . .
16 pounds pf Aroclor - liquid
.
8 pounds of Water .
'. .
.
_
16 ounces of Stearic Acid
* '.
h ounces of Triethanolamine
" ..'
- 4'
The Aroclor la heated to a workable viscosity above 82C (180P) .
and the Stearic Acid Is added and completely stirred in. The
'.
water is heated to 97C (207F) and the Triethanolamine added and.
thoroughly stirred in. After both of these operations have been
carried out, the Aroclor-Stearic Acid combination is poured into
the water mixture while the latter is well agitated and then the
whole mixture is processed through a colloid mill. Good results,
may even be obtained without the use of & colloid mill, provided
the mixture is agitated with a high-speed emulsifying stirrer.
' PLAMBPROOPERS
The Aroelors are not inflammable and when mixed in sufficiently
large proportion with many other materials have rendered the com
plete compound non-inflammable. For Instance, a mixture of about
equal parts of Aroclor 2565 and asphalt gives a resulting compound
that will not permit the spread of flame. Wood may be impregnated . .
sufficiently with one of the higher chlorine Aroelors, such as
M65> that it till pass the most rigid tests now applied to wood .
which haa been treated for flameproofnesa, such as the tests used
by the Forest Products Laboratory and by the Building Department
of the City jpf Bet. lcu*r_^ ... . juxir
anr. .: -Lv;^w
We have not yet found a market for Aroclor in the field ot flame proofing wood because la most cases there the wood Is treated, for flameproofness it is used, indoor# there it is notexposed. teV . .. leaching by rain, ad that'one of the phosphate salts ie generally used,. However, there may be special uses where, these material^.. , are not acceptable .and where the prise of.Aroclor. la justified. ""
____ _____ _________ jvixtrn-'r:; ~;
TOWOLDMONOOOI590
- . . - -- . ..... ...... -* -v........................................... #- 'v- -- 4^- r.** - ,,
*
.
.. '
>
.
' ' "
MOSBABTO CHEMICAL CONFAB?
: ''ib-i-44 ' '*
There is throughout the country e tremendous market for eompQunded
waxes for all manner of uses. It Is very likely that in some of
the applications of these materials it would be deslreble tohavf
them non-inflaanable. It le also likely that the Incorporation of
Aroclor with same other resinous or waxy materials would give other
desirable properties. These applications could probably be worked
out in conJunetic with companies who are now in the business of ,
compounding and selling such materials. There are seme of these
companies In each of our sales territories. . ......
Aroclors *A65 and 5*60 are the most likely ones In this application.
Tests are under way to determine the suitability of the substitu-..
tion of Aroclor 1260 for chlorinated paraffin In the treatment of
paulins and tentage for use by the Army. This is for the purpose
of producing non-Inflammability, improving moisture resistance, .
and mildew proofing. `
'
..
;
The Aroclors are remarkably stable and their superiority In this
respect to chlorinated pareffin customarily employed for this pur
pose Is demonstrated in the following results reported by our
laboratory.
.
.
Light Stability Tests
In order ta be certain that the tests were comparable in every respect, they were conducted by personnel of the A. French Textile School, Georgia School of Technology, Atlanta, Georgia. .
The samples used in these tests had been prepared at Anniston prior to this visit. They consisted of sections of klerbolled cotton
sheeting impregnated with compositions as shown in the tabulation below. Approximately 10 of chlorinated hydrocarbon was applied
to each of the impregnated samples. The chlorinated paraffin used had the following characteristics: -
-
* vr; .
% Cl2 -.... , .......... *3.15
5p.Gr. 9 25/25C
1.183 ' -
TlSOOBity g 210Op I75 333
Foul* Point
-8P
As will bis noted/ several pigments, namely, *203, SbgOj, and
CaCOx, were also spplied to the fabrle. . These pigments were used
In the following proportions:
*
-
.* -
Fe203 10 parts FS203 tod parts chlorine In the chior
inated hydrocarbon,
.
-
Sb203 10 partn8b2Q2 to S'parts jshlerine>^_^
TOWOLDMONOOOI591
......
- ***.
~^ - : W
--.... ~~ MOIBAUTO COMICAL CORFU?
..... ::..
In the tests with the plgoented mixtures, the pigment adhered to the surface of the- cloth and was not very evenly distributed.
The actual testa made at Georgia Tech. Involved exposure for tvo
hours In a Cooper-lewett lamp cabinet, then conditioning at 7Qop
and 65% R.H. for four hours or longer, and finally testii* for
varpvise tensile strength by the grab method with a Scott tester.
The Cooper-Hewefct cabinet had a Ovlare (fused quarts mercury arc)
lamp as the source of eltra-violet light, (to the basis of. dye
fading tests conducted at Georgia Tech, over an extensive period
several years ago, tvo hours' exposure in the Cocper-Hewett cabinet
is roughly equivalent to 20 days' average outdoor weathering. This
relation does not necessarily apply to tensile strength deteriora
tion tests. Judging by the deterioration of the tensile strength
of unimpregnated samples, it would appear that 2 hours' exposure
in the Cocper-Hewett was equivalent to much more than 20 days' cut-
aide exposure.
.
Summarized data for the tensile strength tests were as shown in the
following tabulation:
' ' 1.. '
'
'Impregnation Mixture
. Tensile Strength (X)
` Unexpoaed
Exposed
Hone (Plain cloth only)
_________
55.7527.9
Chlorinated Paraffin
.
n
n A Pe203
.. .
H
It
ft Sb2C3 ft CaC03
Aroc11lor
1254
n
!t R
...
ft Fe203 ft 3t203 ft CaC03
...
Aroc>1lor 12It 60
n if
/ 11 ft
. - - . . . ... '
.-
. ft Fe203 . ft Sb203 -ft C&C03----------
------
57.75 60.9 ----57.0 57.9 T
54.5 60.1 56.2
53.75
59-4 58.0 62.4
59.25
... -
../
15.1 17-75 17.5 18.25
24.0 27.1 24.5 25.9
25.75 30.1 34.9 30.9
Aroclor 5442
".
jcCr^
n it ,'-~:z
ft Pe203 " Sb203 'e^` ' r*:. 4 CaCOJ :
: 60.1
v- 5*5' . - - r.
:? -
. 33.5 ..'-jrc. 34.1 - /. 40.6 '40.9
(X) Units are in. pounds and, except for threer_Instances, the
values shown are. averages of f. tests'.-.
r ' ____
The conclusion from these tests waa that the Aroclora contributed
little, if any, to the dfeterloratleh of tensile strength- of the-- - -
cloth upon exposure toultre-vioiet Ilgbt^wfcereaa'ljWorinated .1
paraffin did appreciably accelerate teterloratlQn under
.
. ......
rcjyrjfe.. ~
.jl.
TOWOLDMONOOOI592
MOIBAUTO CHEMICAL CCKPAMT
10-1-44
conditions. Also, under the conditions of these tests, all of the pigments tried decreased to some extent the tendering effect of the ultra-violet light. This is probably not abnormal, sines the pigments should have reflected a portion of the light rays.
It has been reported that certain pl^nents decrease the heat sta
bility of chlorinated paraffin, thus accelerating tendering of treated cotton goods upon exposure in hot climates. Beat stabil ity tests on all of the impregnation mixtures tried a# outlined above are now being run in the laboratory at Anniston.
Compared vith plain cloth unexposed (100) the hydrocarbon treat ments alone effected the follovlng Improvement in tensile strengths:.
Chlorinated Paraffin . Aroclor 1254
Aroclor 1260 Aroclor 5442
7.55* . 1.35*
10.55* 11.85*
. -
This Increase In tensile strength through impregnation Is compen
sated for in the following calculation.
.-
When the ''Exposed Tensile Strength" is expressed as per cent of "Unexposed Tensile Strength" the following relationship is evident:
Untreated Cloth
Per cent Resistance to Deterioration on Exposure
to Ultra-violet Light
51*9
ChloriItnated It
n
ParItaffin IV
11
at &
*
Fe203 Sb203
CaC03
28.10 29.15. 31.40 31.52
*
AroIct lor 12ft 54 n it
it ` *t . .
ft Fe203
*
at Sb203 ft CaC03
.. .
44.05 45.10 43.62 44.19
Arofct lo r 12ft 60
if m. .. -w 11 tr
^: '
ft Fe203 ft 9b203 ft CaC03
..
... .1.,. 43.36 .....; 51.86 .
. 56.00 : 52.10
AroIct lor 54ft 42 It It It ft
..
` ft Fe203
ft Sb203 ft CaC03
* .
:-
.-
- 55.70 \V
. . 52.05 -
-:
63.53 65.53 -
The advantage of'the Aroclor* im comparison with Chlorinated Par- . . affln as a non-inflammable, waterproof ispregnant for cotton fab-
rlc as measured by resistance to loss of tenfile stren^tlr on.-. : "L
TOWOLDMONOOOI593
fcr : ,
" * v *....... ^ rr- *7;: ----- r*.
*
* ' : - 10-1 M
NOIBAUTO CHBUICAL COMPAR * l
exposure to ultra-violet light is expressed in the following re
lationship, basis equivalent Chlorinated Paraffin treatment as
100J6:
-
Per eent Improvement in Resistance to Deterioration
over Comparable Treatment
with Chiorlnated Paraffin
Aroclor 125* " & 7e203
"4 Sb203 " w 4 CaC03
Average
56.7 54.7 42.1 *0.1
*8.*
Aroclor 1260 * 4 Pe203 4 Sb203 " 4 CaC03
Aroclor 5**2 ` " "4 7e203 * * 4 Sb203 "4 CaC03
Heat Stability Testa
Average Average
5*.3 77.9 78.3 65.3
98.2 78.6 102.2 107.9
68.9 96.7
These tests were made by absorbing and titrating the HC1 evolved
from 20 grams of chlorinated hydrocarbon when held at 175C and
blown with air at the rate of 0.01 cubic foot per minute for four
hours. This Is the method outlined on pages 375*378 of the Aug-
uat 30, 19^3# Issue of the American Dyestuff Reporter, Vol. 32,
Ro. 18. James R. Redmond# Textile Technologist# Jeffersonville,
Q.M. Depot, vas the author of the article.
-
Data for the tests that have been completed were as follows:
Chlorinated Hydrocarbon Composition
. . Jf HC1 Evolved In
.... .
* * hrs. at 175C
20 gms. Chlorinated Paraffin
f ............
20 ns.
. * . / 2.0 gms. Pe203
20 gms.
*
- *
V 10.5 gms 5b20>
20 gms. * . ;i. - ^ 6.3 gms. CaC0>
0.*1
20.00 0,29 0.29
TOWOLDMONOOOI594
V'
* 10-1-M
MOHSAITO CHEMICAL CQMPAIfY
-
Chlorinated Hydrocarbon Composition______________
% HC1 Evolved in 4 hrs. at 175C
20 gms. 20 gms. 20 gms. 20 gms.
Aronclor w m
12f! 60 N IV
/ 2 gms. Fe203 / 2 gms. Sb203 / 2 gms. CaC03
0.002 0.02
0.005 0.01
20 gms.
20 gms. 20 gms. 20 gms.
AroIcI lor 5442 It It
IV VI
12 gms. 7e203 / 2 0ns. Sb203 / 2 gms. CaC03
0.00
0.00
. 0.02 0.02
These data clearly demonstrate the markedly superior heat stability of the Aroclors as compared to chlorinated paraffin. Particularly significant Is the accelerating action of Fe203 on the decomposition rate of chlorinated paraffin. Ho such accelerating action vas noted
vlth the Aroclors.
While In most of the tests with the Aroclors our titrations indi cated the evolution of HC1 ranging up to 0.02$, the titrations vere so small as to possibly be vlthln the range of experimental error.
At any rate, ve are quite sure that 0.02$ HC1 evolution represents the maximum HC1 loss under the conditions of the tests.
Chlorinated Hydrocarbon Mixture ,_______________
$ HC1 Evolved in 4 hrs. at 175C
20 gms. Chlorinated Paraffin and 2 gms. Zinc Borate #2167
20 gms. Aroclor 1254 and 2 gms. Zinc Borate #2167
12 gms. Aroclor 5442 and 8 gms. Trlcresyl Phosphate
12 gms. Aroclor 5442 and
8 gms. Trlcresyl Phosphate and
2 gms. Fe203
. .L.
12 gms..Aroclor 5442 and
8 gms. Trlcresyl Phosphate and
2 gms. Sb22...............
....
12 gms. Aroclor 5442 And
;
8 gms. Trlcresyl Phosphate and
2 gms. CaC03
-
12 gms. Aroclor 5442 and 8 gms. Trlcresyl Phosphate and 2 gms. Zinc Borate #2167 m_
.
.
*. ..
15.6 0.01 0.02
0.00
0.01
0.00 ` .
0.01
Again It vlll be noted that the Aroclors are far more stable than
Chlorinated Paraffin 1*^ the presence of. Zinc Borate, .. ..
..
TOWOLDMONOOOI595
. ,-- . .
` ' ` :
15-1-4%
r MONSANTO CHEMICAL COMPANY
HEAT TRANSFER MEDIUM
.
.
Aroclor has been used for a number of years at Anniston as a Heat transfer medium. It Is now employed as such In the HB-40 plant.
Company (075050) used Aroclor as a heat transfer medium In main
taining a molten lead bath In which they soaked 1% Inch armour
piercing projectiles. They operated one unit using Aroelor and
another using Dovtherm. Both of these units were used for several
years. They then discontinued the use of Aroclor after discover
ing corrosion in the Aroclor system, which did not occur in the
Dovtherm system.
.
^
*
A company developed some equipment for heating pyrites in which
they Intended using Aroclor as the heat transfer medium. Since the equipment was never sold commercially, none of these units involving Aroclor are now in operation
Many people considering Aroclor as a heat transfer medium gave it
up either because it would not stand the temperature they required,
or on account of fumes ccaning from the Aroclor, or because it cost
more than oil normally used for this purpose.
.
Favorable features to the use of Aroclor for this purpose are: <
1. Liquid at room temperature.
2. Does not oxidize.
\/
5. Has nearly twice the specific heat of petroleum oils generally used for this purpose.
'
4. Non-inflammable.
-
HYDRAULIC FLUID
Company (576,450) operating a high pressure steam-electric gener
ating plant use Aroclor 1248 as an hydraulic medium in their gov
ernor system. They do not use it as h lubricant. The Aroclor 1s
used instead of oil, merely because of its non-inflammability.
When oil is used in the governor system. It' la customary to use the
same oil reservoir, both, for the lubricating and governor systems.
When Aroclor is used in the governor system and petroleum oil in
the lubricating system, it is necessary to segregate the two sys
tems and use separate pumps for the lubricating and governor eye-
temS. .
.
;v
~ be-- h
Vestinghouse have been the principal promoters of the use of Aro-
olor in the governor system as a result of having the oil .in a ,:~
( governor system catch fire in one of the fMrsey Centfal.Light aad :
Power Company's stations while Vestinghouse engineer* V$re working
with the unit, .
-
BBRN0D2032 ..
TOWOLDMONOOOI596
i*
10-1-44
' MONSANTO CHEMICAL COMPANY
BEAMSls
Company (104460) has obtained sane Interesting results with baketjon enamels containing Aroclor 1254, Acrylold Resin and Tricresyl Phosphate, pigmented vith Titanlias Dioxide and Zinc Oxide. The enamel is baked on at 135C (275P) They have found that Trioresyl Phosphate aids the Aroclor on baking, giving a hard surface..
This same company has found that mixes of Aroclor and Vistanex (No. 6 B-80 and B-100) or Aroclor and Vixtac (No. 1 and No. 2) give Interesting properties somevhat like shellac. They state
that these products have good adhesion. - .
LACQUERS
.
. Ve have a very good general line-up on the use of Aroclor in lac quers in the booklet P-115 which ve have published for distribu tion. This booklet gives the limits of compatibility of Aroclors 1254 and 1262 in Nitrocellulose lacquers. Since this booklet has been published, a number of companies have started using Aroclor
1242 in special flexible lacquers, such as are used on high tenslon cables, etc. The compatibility limits of Aroclor 1242 are higher than those of the higher chlorine Aroclors so that it is possible to Incorporate enough of the Aroclor to give it extreme
flexibility. You have the formula for Aroclor Lacquer No. 34 which gives the details of the use of this Aroclor in cable lac quer.
The work done in our laboratory using Aroclor in lacquers indi
cates that ve get somevhat less chalking vith the Aroclor lacquers
than vith those made up by other formulae. Ve get practical free
dom from checking and cracking and, ve believe, better color re
tention in the white and light colored lacquers. These are impor
tant considerations in lacquer manufacture, and Aroclor should be
given much more consideration from hov on for general use such aa
an automobile lacquer, etc., than it has received in the past
because of the vising prices of other resins vhich are generally
used.
'
- Ve have a number of customers vho use Aroclors 1242, 1254 and 1262 ,
in the manufacture of lacquer. : :
J
.
Lacquer Formulatlon'Chart
:
TOWOLDMONOOOI597
MOKABTO CB9IICAL CCKJAXl /
Volatile Constituents
\ . ..
.\T-*" v7;-.:
M444
1. The alcohol constituent 2. The eater oonatltuent 3- The hydrocarbon oonatltuent
Finished Lacquer
'- '
Z per cent of the non-volatile
.
(100 - Z) per cent of the volatile _
. .. ~i
. .
The percentage Z, of the non-volatile or film-forming constituents, nay vary between 20jf and 30% of the weight of the finished lacquer
Won-Volatlle Constituents
As has been shown by the table, the non-volatile components of a lacquer consist of a resin, cellulose nitrate and a plasticiser or . softener. For the resin, sane one of those of synthetic origin may be employed, or a natural resin such as Qua Danner may be used. Gum Dammar Is a generally used resin in lacquer formulation, and It can be taken.as the number one component. The number two component
Is the cellulose nitrate Itself. It Is alea known as nitrocellu
lose, Pyroxylin and "PZ." To the Industry In general it la "cotton." It can be purchased In two kinds, the AS and RS grades. The latter
grade la the one that la chiefly used by lacquer manufacturers.
The initials Indicate a difference in the method of manufacture,
AS meaning that the cotton Is alcohol-soluble, and RS meaning that
it la regularly soluble.
.
j., .
Both grades are usually bought wet with denatured alcohol.' The
viscosity of the cotton- la another determining factor with regard
to Its use. The cotton that.la commonly employed by the Industry
has a viscosity of one-half second and la known aa "half-second
cotton." For the third component dibutyl phthalate, tricresyl
phosphate or castor oil may be used. .
;'
`
At this point an explanation of the terms "plasticiser* and "sof
tener" becamea necessary. The average lacquer technologist uses
these terms synonymously, and for this reason they have come to
mean almost one and the same thing 1 this Industry./ Btrictlj/ -
speaking, a true plasticiser, should be a solvent for- tbe "cotton"
and the resin. In addition, it should have a low vaporisation
`
loss and should confer such properties aa flexibility pliability,..
and durability on the lacquer film. Both dibutyl phthalate and - . ~ ^
tricresyl phosphate meet these requirement**,. Castor oil*'an the
other hand, does hot, tn that it Is only a partial solvent for ...... .
"cotton." It does, however,'give to the film the qualities al* W;
ready mentioned. In short, it exerts a. softening effect - hence.7_zl_:-_--
the name "softener." The difference;-'then, between ^ plastleiSep.
and a "softener" is that the fomer ls ,a true solveatfer the
^ '
-
t?TOWOLDMONOOOI598
'
NOBAMTO CHEMICAL COMPARf
' ' > -
non-volatile constituents of a laoquer, while the lattar la a nansolvent, or, at beat, only a partial solvent. Castor oil la typi cal of this latter class and is widely used as a lacquer "softener."
Volatile Constituents
...
The volatile constituents fora what Is knows as a balanced solvent
mixture, the purpose of which is to be used as a solvent or thlnney
for the non-volatile constituents. Tbs components of this mixture
crust be in such a proportion to each other so as to insure a uni
form evaporation rate when the lacquer film dries, and also to make
sure that no precipitation of the "cotton" will occur at the time
of thinning.
- -
.
.
The number one, or the alcohol, component Is generally composed of
ethyl alcohol - 950 and butyl alcohol. The ester component Is made
up in general of ethyl acetate and butyl acetate, while the hydro
carbon component usually consists of seme compound such as toluol
or, for special lacquers such, as cable dopes, benzol.
Finished Lacquer
** -- .
. -
i ,
'*
The finished lacquer is prepared by taking a given weight of the non-volatile constituents and dissolving them in a given weight cf the volatile constituents. .
Competition
The question of competition will have to be viewed from two angles; first with regard to the Aroclors as resins, and second with regrr.l to them as softeners. Since the Aroclors have more the properties of softeners than of resins, the softeners are nearly competitive with the Aroclors than are the resins.
Competing Resins - Synthetic
flame Amber ol
Number 80l`- '
Manufacturer
The Beslnous Products & Chemicals Cc. ............. Philadelphia, Pennsylvania
Bakelite
Bakelite Corporation
' v "'
Mew York, flew York - -
Beckaclte
Glyptal ..
Levisol
(1110) (1U4) ^
1202 *
Beck, Koller A Company, Ine.
Detroit, Michigan " i--.-- . f atr' '
~ _
General Blectrle Company
.
Schenectady, Mae York ' 7
7
. #. ` '.rji . -- -:-h$
- dm
. - - -* `
John D. Eevfi, lacT'**:*77 Providence, Rhode Island
TOWOLDMONOOOI599
MONSANTO CHEMICAL COMPANY
10-1-44
Competing ReaIns - Synthetic
Name
Number
Manufacturer
Paraplex*
ili%
The Reslnoue Products & Chemicals Co.
Philadelphia, Pennsylvania
.
Re zyl
American Cyanamid & Chemical Corp.
New York, New York
`
Rezyl Balsams -
Teglacs
-
American Cyanamid & Chemical Corp. New York, New York
*
American Cyanamid & Chemical Corp. New York, New York
Paraplex can probably be conaidered a softener as veil as a resin.
Competing Resina - Semi-Synthetic .
Name
Number
Manufacturer
Ester Gum
None
(One of
the most generally
used resins.)
There are many manufacturers
Natural Resins
`
Gum Dammar
(Batavia)
Imported - obtained through brokers
(Singapore)
Competing Plasticizers or Softeners
Name;GradeTrade NameManufacturer _
Dibutyl Phthalate* -
- Monsanto Chemical Co. St.. Louis, Missouri
Tricresyl Phosphate* -
...
._
- Monsanto Chemical Co. St. Louis, Missouri
- - `
.Kronitex ..
Kavalco Products, Inc. Nitro, West Virginia
- Lindol
Celluloid Corporation
- Newark, New Jersey
Abalyn
: (A roein produet
. Hercules Powder Company
' - recommended for
. - Wilmington, Delaware
lacquer fonsulatlon)
' ' `.
..
.*. '3r*
: *> 'i.'-rr-
TOWOLDMONOOOI6OO
MDSAirro CHEMICAL COMPANY
* 10-1-44
Competing Plasticisers or Softeners
Name
Grade
Trade tame
Manufacturer
ADM-100
(A modified linseed oil for lacquer formulation!
Archer-Daniels Midland Co, Milwaukee, Wisconsin
Castor Oil (Baker's)* Number 4
.. Humber 15 Rumber 16 AA
Blown The Baker Castor Oil Co. Blown Jersey City Rev Jersey
Blovn Unblown
Spencer-Kellogg Oil
(A modified castor Spencer-Kellogg & Sons
oil for lacquer Buffalo, Rev York
formulation)
'
There are other manufacturers of these products - this list is
by no means complete.
-
In listing these products, only those that are in more or less gen
eral use have been Included. There are some notable exceptions, hovever, in the cases of such materials as Abalyn, AEM-100 Oil, and Spencer-Kellogg Oil.
The materials listed in these tables must not be thought of en
tirely as competing products because they may be more important
as aids or auxiliaries in co-development vork with the Arodlors.
In fact, it is believed preferable to regard them more in this
light than as competitors.
'
Advantages
.
In thinking of any advantages the Aroclors may have, the statements made in the final paragraph under "Competition" must be borne in mind. It is preferable to confine oneself to a discussion of the
outstanding properties of the Aroclors, for it is believed that it is only through the.development of some specific property that progress is going to be made. _ .
The properties of the Aroclors that should be emphasised are: :
1.* Lov vaporisation loss
2. Pale color___
3.. Adhesion
-
4. Chemical Stability
|
. :"
* - -
'
.. ' -
a. . to light b. to water*. acids and alkalies . . . `
TOWOLDMONOOOI6OI
MOKAirrO CHEMICAL CCMPAlfY
10-1-44
5. Han-inflasnnabillty
6. Non-corrosiveness 7. Solubility in commonly used lacquer solvents
A resume of the properties that Aroclors Impart to lacquers and
the types of lacquers for vhlch they are recommended may be given
briefly as follows:
''
In a Dammar-type lacquer the plasticiser-softener combination, such as the usual dlbutyl phthalate-castor oil combination, nay
be advantageously replaced by an Aroclor alone. The resulting lacquer is less subject to checking and cracking on outside ex
posure and retains its gloss. (
Aroclor 1262 may also be substituted entirely for the resin In
certain types of lacquer. The clear lacquer, so produced, is practically colorless and provides an excellent base for white
enamels. Such enamels, however, do not withstand weathering as well as those containing Dammar in addition to the Aroclor. -
The advantageous properties of the Aroclors in imparting added
weather resistance to properly formulated lacquers may be traced
to their resistance to the action of sunlight, to their perman
ency in the film, and to their extreme chemical stability. The
Aroclors do hot oxidize, "dry," or harden. The Aroclors.are un
affected by dilute acids`and even by hot caustic solutions. They
are not subject to polymerization, rancidity or other change, as
far as is known.
.. ` , .
When added to a nitrocellulose solution, the Aroclors reduce the viscosity slightly. This change in viscosity takes place at once and no further change due to the presence of the Aroclor occurs on several months' aging in closed containers.
By virtue of their high refractive index, they impart apparent
depth to the lacquer film. Aroclor 1262 has adhesive properties
and the lacquers containing it have good adhesion. Lacquers con
taining the Aroclors dry normally and give a hard, non-tacky,
durable film of excellent gloss-
.
'.
,,
Certain lacquer technologists have found that a lacquer contain&ig
Aroclor can be polished with a minimus of rubbing and, furthermore,
that the Aroclor seems to impart a harder finish to a lacquer film
than oils, trlcresyl phosphate, or dlbutyl phthalate. It has also
been reported that properly formulated lacquers containing Aroclor
show no tendency to *spev* or "sweat out* when buffed. - - *
~
In addition to the properties of general interest,: other proper ties of the Aroclors arc of t-.luc in formulating lacquers to fit
special requirements. Aroelors/1254, 4465, 5460 and 126? do not support combustion, and when present in nitrocellulose films they
BKT GBRN002038 ' "isaas;
TOWOLDMONOOQ1602
NOIBAIVTO CHEMICAL COMPAJVZ
10-1-4%
retard the rate of burning. The Aroclors retard the rate of trarts-
fer of moisture and of gases through a nitrocellulose film, and by
virtue of this fact have already found extensive use in protective
lacquers far application over those types of electrical insulating
materials, such as rubber, that deteriorate rapidly In contact ;
vlth oxygen, ozone, moisture or other vapors.
h
Procedure
t
-f
Upon visiting a lacquer company, every effort should be made to
see the chemist in charge of formulation or production. In large
companies the director of research should alvays be seen. As a i
general rule, a great deal vill not be accomplished until these ;
respective Individuals are seen. '
.
.
i'
A complete discussion of the properties of the Aroclors should be
given, emphasis being placed upon the possible formulation of a
new lacquer vlth sane one of these properties as the background.
. '
When discussing the use of Aroclors in lacquers, the salesman
should remember that the Aroclors are not solvents for nitrocel
lulose and that for this reason an excessive amount of Aroclor
must never be used In the formulation of a lacquer.. The limiting
percentages that can be used for successful results have been
carefully worked out by a large number of experiments. The few
simple rules that must be followed in formulating lacquers with
the Aroclors are emBocTied in a booklet entitled "The Properties
of Two Aroclors of Special Interest to Manufacturers of Lacquers."
Copies of this booklet may be had on application to our sales
offices. It is recommended that the salesman offer copies of this
booklet and the bulletin "Plasticizers & Resins - Organic Division"
to interested lacquer manufacturers.
..
.
*t
Attempts should be made to determine what particular lacquers a
manufacturer specializes in and what problems he is studying at
the time of the call.
.
Aroclors have fair or good compatibility vlth nitrocellulose,. Fora-
var, Butvar, vinyl copolymers, polyvinyl acetate, poly-styrene,
chlorinated rubber and ethyl cellulose. In general, the liquid or
semi-solid Aroclors act like true resins. One principal,value is,
their chemical inertness. Where great flexibility is to be ob- .
talned, it may be necessary to employ auxiliary plasticizers.
Soma of the exceptions are in chlorinated rubber and in ethyl
cellulose where flexibility or hardness may be varied simply by
*
selecting an Aroclor of the proper physical Characteristics.
.
The liquid Aroclors such as 1242, 1248 or 1254 vill greatly in
crease flexibility but will cause softness. . 'The semi-solids such
as ic60 or 5442 will impart same flexibllity.irlthout the marked.'
softening effect. The brittle, resinous Aroblors Such'as 4465 or
5460 produce very hard compositions vlth excellent adhesion and .
'
TOWOLDMONOOQ1603
J* ' -*
.... - CS*
... JUCAlfTO CHEMICAL COMPART
- la&'-M '.X
weathering quail tie*. If a single Aroclor does not Impart this de
sired combination of properties, usually sobm mixture of Aroclors
will do so.- Zt would seem that In polystyrene molding eompoaij-
tions, the resinous Aroclors could be used as a flux or flow pro
moter at molding temperatures without causing softness and flb$ at
normal temperatures. 3ose mixture of Aroclors or a combination
of an Aroolor with another plasticiser either solid or liquid \
might be required for this purpose.
,
. '`
Of course. It Is well knovn that for alkali resistant coatings, ;
combinations of Aroolore (1254-1260 and 5460) with chlorinated
rubber have been used for a long time. At the present time, the
use of equal parts of Aroclor 5460 and ethyl cellulose is being
pushed by Company (331850) as a weather resistant coating. Sim
ilar coatings of low viscosity polystyrene and Aroclors would
probably be of value.
...
ABMY-KAVY ABROHAPTICAL SPECIFICATION
LACQUER - CAMOUFLAGE
:{
AR-L-21
V
TABLE IV
Control Formula - Clear Vehicle
:
weight
Weight
IFs. per
Ingredients
Percent 100 gal.
Volume
gal.per 100 gal.
Paraplex RO-2
' (100*) 11.1
90
m
Amberlac B-94
(80* In xylene) 5.6
A.-oc?.or 5460 __________ :____ (100*) 4.3
45 > 35
'w
Ethyl Cellulose(3 to 4 sec)(100) Cellulosfr-Mtratel^g iS^thyi*
axacholj
4.3 9.4
Ftryl Alebioi Ethyl Acetate Butyl Alcohol
.*. . ...%. .S'Jjatrxri?. ~.
- * -
`
#' * ` --
.*
. * 4.5 12.4
35 'm - '
... 75
zste __ ` --?&& ---v 4 '
.
.
.
,- 5 . 15
Butyl Acetate /
* i-.
atomtie* Petroleiai BbphtZHS'
Type 1, Grade B
v "
* 22.4
- -v - -
* : '
22T.^~';:
-- --
--. ,v_\-
25'
piSr. y
tGBRN002040 ______ , ^sSaSi
TOWOLDMONOOQ1604
.'
''
MONSANTO CHEMICAL C0MPAJI7
10-1-4* ; -
It Is Also of value In other resins where a highly alkali re
sistant plasticizer la required. Papers hy Bowran. Paint .
Technology (reference for December 1936, dated January 1937)
Indicate many possible applications for the Aroclors. Sales,
to lacquer trade at present- are confined to specialty manufac
turers.
1.
The compatibility of Aroclor 4*65 in 1/4 second nitrocellulose
is indicated as:
.
.
1. Between 24.2$ and 26.5$ by inspections for blush in
thin aged films.
' .'
2. Between 13.7# and 16.6# by inspection for loss of
gloss in thin aged films.
.
-
The presence of a mutual solvent such as dlbutyl phthalate raises
the compatibility.
.
The formulation of a flexible lacquer designed for oven drying
is given as follows:
-
Non-Volatile 25# Volatile 75#
15-20 Sec. R.S. Nitrocellulose Trlcresyl Phosphate
.Aroclor 1242
e
^Benzol Alcohol Ethyl Acetate
J`
32# 40# 28#
62# 22# 16#
This formula is intended for application followed by oven drying.
Air drying at atmospheric temperature causes blushing. . A modi
fication of the volatile portion is suggested when air drying is
used.
-
'
.
Volatile
'Alcohol'
|Ethyl Acetate
,Butanol Butyl Acetate Toluol
6.4# 6.4# 6.4# 30.8# 50.0#
Experiments on flock insulation and lacquers for aircraft indi
cated Trlcresyl Phosphate as a choice over Aroclors in Ethyl
Cellulose lacquers, especially since there is no tendency to
settle out when Trlcresyl Phosphate is used. Aroclor is more
effective Inflame retarding, however.
.
Stop-Off Lacquers
. - *
. . . _ 4
Rather detailed information ,1s given, la the Monsanto (Organic
Products Division) Plasticizers and Begins Booklet on the preparatlon of Nitrocellulose lacquers containing Aroclors'. A ......... --
TOWOLDMONOOQ1605
'' , MONSANTO CHEMICAL COMPANY
.
10-1-44
suggested formulation Is as follows * .
r *.
1/2 second Nitrocellulose, Dry
Aroclor 1260
..
Tricresyl Phoenhate
`
Santicizer B-lo may be substituted for
Tricresyl Phosphate
100
80-70 >9-70
'
If the Nitrocellulose itself does not have sufficient resistance,
a composition of Aroclor with a chlorinated rubber. Ethyl Cellu
lose or a Vinyl Resin again using. Aroclor is suggested, and if
the flexibility is not sufficient. It can be improved by the ad-
dltion of a small amount of one of the liquid Aroclors such as
1242 or 1254, although again Tricresyl Phosphate or Santicizer
B-l6* could be used.
,
In coatings, as a general rule, the hard resinous Aroclors will produce very hard and very resistant compositions, but these will be brittle. . The liquid Aroclors will tend to produce flexibility but may be lacking ecaevhat in adhesion. It is for that reason that ve have suggested Aroclor 1260, which is about half-way between and vill produce a combination of flexibility end adhe sion. It will be' obvious that hardness can then be increased by the addition of a harder Aroclor such as 5460 or the flexibility, can be increased by the use of a liquid Aroclor. The Aroclors themselves are unaffected by acid and alkali.
Stop-Off Waxes
-
..
The characteristics of a stop-off wax should be as follows:
a. Tightly adherent to metal surfaces.' '
b. Should not be removed at a bath* temperature of l6oP.
c. Should not be'affected by the acids or alkalies of
electrolytic baths. . '
d. Should prevent electrolytic activity on the surface
covered.
`
e. Should be capable of removal by solvent vapor phase
. cleansijig baths, by gelting in boiling water, or
ordinary cleaning solutions. .
Suggested compositions areas follows; 7
Msthide (Monsanto Merrlmao)
40$
Aroclor 5442
-, 7 . - 7 * - 6o
Softening Point
- 118C.
-
Methide (Monsanto* Merrimac) Aroclor 4465 ^
2ojt . 80J*-
108CV :-v-
An attempt was madeto use tfiesd'compositions in solution form by dissolving them in turpentine. This was not particularly '
^i%sasibS3!4e*Trjv
6BRN0020M2
TOWOLDMONOOOI6O6
. - jV --;.- J^ar A V
v * 1Q-1-AA
MQBAKT6 CHEMICAL COMPAH*
(
successful since at room temperature the degree of solublilty
was less than 12$. It night be possible to use a 25$ concen tration of van in turpentine at 50-75 0, painting, the natal J
surface with the hot solution.
.
l.
'..'
\
**
'
#*'
.
*
. PAIBPTS
*~ :..
:r *
*
. v- .
''
Paints containing Aroclor have shovn remarkable durability*far
better than any other .paints against vhich they vere tested.
One serious drawback, however, is that paints containing Aroclor do not brush as readily as the normal house paints. Paint manu facturers Interested in quick drying points should be encouraged to try Aroclor.. Under war conditions there is great interest in the manufacture of fire-proof painting for the interior of ships. Aroclors should be a definite contribution to their formulation.
Aroclor 5^60 is successfully used in camouflage paint where It
imparts flameproofness. -
' ... ~ '
VARWISHB3
7 ./............... .
( There has been only a limited amount of work done in our labora tory on the subject of Aroclor in varnishes and frcm that work it
has been concluded that the most likely field for Aroclor in varnishes is in conjunction with some other resin such as Ester v_ Gum or Dammar, or one of the other commonly used gums, since the
use of Aroclor alone has, in our experience at least, given a
tackiness to the film.
r.
Aroclor 1262 mixed with East India Gum and but with naphtha fur
nishes a varnish base.
*
The Aroclors may be used in alkali-proof varnishes by incorpor-
atlng them as a sold cut or as a chill back -- and for the pur
pose we recommend. Aroclor 1262. The Aroclor may be said to
function either as a resin or as an oil. In other words, by the .........
addition of the Aroclor, a'short oil varnish .takes on many of
the physical characteristics of a long oil varnish.- Oar work
.
along. thi% line has indicated that the best procedure is to cook
.
* (in the usual.mannerV nsIng aa a resin base a pure phenolic resin - .
but using* only half the. usual amount of china-wood ollr . Vhen the .
varnish attain* proper-body, the Aroclor may be added directly ;
as a chill* back and the. varnish then thinned te) the usual manner. . .
Since Arocior l262 iii a;.SemI-s61id' resin,' It la best heatqd until,
liquid before lntroduclng aa the chill back.'
~ **
An optional method.i*. to dissolve it in the 'tUaner<*h&d tid la
C the usual thinning opemtioar 7'This wai^wprfcedo^aahpoes ibis' means of extending the euppHefr^of china-wood old. - In.ether... words, it acts.M._-Pi^--f^ti.twte s^JLt|^_as^.,re*in sub-.........
BBRN0020M3
TOWOLDMONOOQ1607
MOJOAJfTO CHEMICAL COM PAW
-
In regard to the alkali resistance, ve have found that provided the other materials have, of themselves, considerable alkali resistance, then the Arcolor will add to that resistance. It Is not possible, however, to use a resin such as limed rosin or ester
gum having poor alkali resistance and Impart high alkali resis tance by the addition of the Aroclor. . - - .. ; -
Aroclor 1262 can be used to replace up to 500 of the china-vood
oil in varnishes.
;' ' *
v
1. If ester gum, rosin-., or other cheap resin is used, the varnish will be suitable only for interior work.
2. If a good 1000 phenolic resin Is used, the varnish
will be satisfactory for exterior purposes.
.
Varnishes containing Aroclor 1263 are not superior in quality to
similar varnishes made with tung oil alone, vitb the possible ex
ception of a very slight improvement in alkali resistance,.flexi
bility and adhesion In some formulations.
_
Varnishes containing Aroclor 1263 soften at lover temperatures
than do varnishes employing only tung oil, and "so are more sub- -
ject to "printing" and marring vhen warm. ...
'
The advantage of Increased flexibility of Aroclor varnishes is lost'at lov temperatures due to embrittlement of the Aroclor.
Because Arodors weigh more per gallon than china-vood oil, they
Increase the cost of varnishes (which are sold by the gallon)
even if put at the same price per pound as the oil.
.
LUBRICANTS -
\
An outstanding service Is performed by Aroolor 125* as a lubricant
for high pressure air compressors operating at 4400 pounds per
square inch pressure. Besides avoiding flammability, it is
claimed that the- lubricant IS superior to oil, no corrosion de
posits result, and there is no excessive.wear bn the equipment
(Company 15850-). . '
`
' ... . . ' i'.
Company (235950) is using Aroclor in a 'special drawing'compound.
Company (5*1370; tested Aroolor 12*8" in one'of their pumps operat ing at 2500 pounds pressure with the.following results: . !
Compressibility change is 0*30 compared to 0.50 for petroleum-oil. The wear rate of the pump was measured by observing the slip of the pump at Intervals during the endurance run. Inspection of the
pump showed the wear to hsve: occurred on the. piston hole sails in . the cylinder and on the hardened surface of~ the pintle /the sur
face of the pintle felt wavy - not smooth/-' 4 m? rate of 220 per ~
1000 hours was found to exist ^_ _ The wtsaos Itf siape of A^
8
was poor. ....
.--W-V
'
-r A'-
TOWOLDMONOOOI6O8
10-1-44
f WHBAHTO CHEMICAL COMPAXT Ths conclusion of these testa is reported as follows: Aroelor
1248 Is not a rerj satisfactory fluid for general use in oil gear
pumps at 2500 pounds per square inch. It is expensive as the
pump requires special paint os the Outside and inside; the oper
ating range is narrow and the wear rate on the pump tests vaa 22%
per 1000 hours at 100F and 25 pounds pressure.
'.
Our experimental work in using Aroelor as a lubricant in steam' turbines was not successful, due principally to the fact that the Aroelor is of such high density that it picks up any bit of grit that nay be in the' system and floats it up in the bearing.
Petroleum oil having so much lover density allows most of these ' particles to settle in the bottom of the reeervolr.
United States Patent #2,245,649, assigned to Celluloid Corporation,
describee a steam turbine lubricant consisting of 50-parts of
-
chlorinated diphenyl and 50 parts.of triaryl phosphate. .
.
E. P. Lubricants ` `
.
' ...
Much attention is being given by lubricating men to the matter of
increasing the film strength or load carrying capacity of lubri cants, particularly so as to be able to use smaller gears for a
( given load
There are a great many such lubricating compounds now on the
market. As a class they are called "Extreme Pressure* or E. P.
Lubricants.
..
.
.
It is well accepted in the lubricating Industry that by the addi
tions of certain elements as Chlorine, Sulphur and others in the
proper form to a lubricating oil, a certain chemical combination
takes place with tbs iron or steel metal bearing surfaces. These
surface compositions tend to prevent seisure of the rubbing sur
faces under extreme loads and under which loads, if the sole
lubricant vaa a pure, mineral oil, seisure or scoring would result
at once through film failurei
...
.
In attempting to discuss Aroelor as an extreme pressure base. It
is very difficult ts evaluate its comparative load-carrying
'
capacitiet^with,other extreme pressure bases,, such aa lead soap,
active suiphur, saponifiable oils, sulphur chloride, etc., without
actual results from exhaustive tests not only of the various
E- P. testing machines',, but also from actual service under normal
.operating conditions* .It Is recognized by the. lubricating Indus
try that results obtained on testing machines; such as Almen
machine, Timken machine and others, mean w*rylittle unless the
results are.correlated and proved by service- conditions.* IV is _
true that ftt the past Aroelor has been tested^as an.Et~ base- `
on the Timken machine.at Timken toller tearing and oas the General
_ii
* * , - ".r-
- - -ars
" `
TOWOLDMONOOQ1609
. - * ; -
10-1-44
MONSANTO CHEMICAL CQMFAJff
.'
\`
Motors machine at Central Motor* Beaearsh, and In each case the
Aroclor addition has shovn a marked Increase In load carrying
capacity.
:.
-
Several companies are purchasing Aroclor today for use In X. P.
Lubricants, but Indications are that they sometime add other elements along vlth the Aroclor to achieve commercial results at
a lover price. Since ve have never run service teste on the Aro
clor ourselves and the fev companies purchasing Aroclor are naturally very reluctant to divulge their experience along vlth vhat other cheaioale, If any, they are using In conjunction vlth
the Aroclor, the beet that can be done Is to offer comnents by several of the companies vho have tested the Aroclor and possibly give a general interpretation' or suggestions as to vhere it might find more general present day application.
. ''
*
Top Cylinder Lubricant
.
-
'
Recently the practice of putting a lubricant In motor gasoline
has became quite general. This Is, of course, to lubricate the
top section of the cylinder.
.
Ve have two customers vho purchase Aroclor regularly for use in the top cylinder lubricant, which they make and sell.
Ve do not know the function of the Aroclor in this use other then that.these customers tell us that It prevents the deposit of
carbon on the valves. Ve understand that they use a relatively
small percentage of Aroclor in the lubricant.
One of these customers uses Aroclor 1248 and the other uses
Aroclor 1154.
.
Ve have* done very little work vlth the Aroclor as a top cylinder lubricant but vould suggest that Aroclor 1246 be used In small percentages. This Aroclor will be found completely soluble In low viscosity oil and should not eause any appreciable difference
in Its cold test. This Is often added to the-gasoline to achieve
top-cylinder lubrication.
Company (755900) obtainedr excellent results using Aroclor 1254 -
on a bearing test,; operating la straight Aroclor at. 255-260? . (124-129C) for two weeks. Muoh less carbonisation and deccaposition than vlth the usual spindle oil under the same conditions.
Compatibility of Aroolors vlth Cellulose Acetate >.
Experimental York. The compatibility Halts of^Airoelor: 1562 vere ' determined vlth five grade# at cellulose acetate, far these
TOWOLDMONOOOI6IO
....
..
parses `*.#. 2.fi. ,,
: . V,~. 7 -..-- -.-
V.^Sfe^'SSWfiMR
-?'ra mr^gyv-t y.*f'"r^rr-
rty -.-a*
* ;`:v-
a;1
/v.
--
;-\z*
*^
.
f
J* *vy-"-T"'
r . * WJBARTO CHEMICAL CCHPAHY
#-'--,->*. .' .- *V.
- - .
' - - ' 1 ,,
cellulose acetates the Unite were as follows:
* J,V . ?v. V
Sastmah Cellulose ` Acetate Huber -.
702$ 7026 '-ISIS
.. *,,
10246
Compatibility LimitodT Aroclor 1262 (per centT
Between 1C.0 Ind 13.6;
* ' %v . U *
Between 16.2 and 17-9;
Between 13.1 and lo.5:'5^v:-'J/-
Between 17.8 and 19.7 - ' -
Between l6.4 and io.l ' T' ,;
-------a
These figures, as well as all the compatibility Units'given In
this report, refer to the Unite as determined or* thin films .
dried slowly In dry air and deposited.from solutions containing,
as is customary, 0.1 gram of "solids* per cuble centimeter of
solution. The solvent was a mixture of 80% by weight of*ethylene
dichloride and 20)1 of alcohol (denatured, Formula
-
Another solvent mixture comprising 33-3% acetone, 33.3^ ethyl
.
lactate, 16.7% alcohol and 16.7% ethyl acetate (all percentages . r*''
by weight) was less suitable than the solvent given above; and . ..H
gave lower compatibility Unite in the cases tried. .
'V-U *
Tne compatibility Units of several Aroclors with one cellulose
C acetate (#10246) were determined. The observed limits were as
follows*
` ~-
Aro^clor Ho. ` . .'. ^Limit (Per cent):^ ' j. jp*-- _
" V 1242
* From 25.9 to`28.7'~
--
1254 :
* ' From 25.T to 29.1- -
. 1262- yjjS". ' , From 16.4 to 18.1 . . ^ ' /
: " 4465 -".V-i-.: *: ; Prom 14.2 tn 16.8 ' v.'?s
v 5465 r -Fru 10.1 to 13.0
The ternary systems, eanprlslhg s' cellulose acetate, Aroclor 1254,
and a common plasticiser, were investigated. .t\ -
:
.
. ..... V-.- 1,
> * #
* . jg \r ' 7..:;-.-
'rV r.
The constants. Ot the Cellulose acetatee, as given by Bastman
Kodak Ccnpany/ are am follower
'
:__ .'-7$::,*-. \Gelluloee7:
- Acetate Wo,
BBRN002047 l| TOWOLDMONOOQ1611
M033AKT0 CHEMICAL COMPART
10-1-4*
Conclusions
The compatibility limit* of various Aroclors in a specific cellu lose acetate and of one Aroclor is various cellulose acetates are comparatively low. The type of solvent employed affects the ob served limits, -the solvent which gives the more favorable results
being the mixture of ethylene dlchlorlde and alcohol. The com
patibility limits of the Aroclors in oelluloee acetate are, in
general, more difficult to determine and less readily checked than the limits in nitrocellulose. The actual observed limit apparently depends upon the rate of drying, the thickness of the deposited film, the humidity of the air, and the solvent employed.
In the tests of compatibility made by Eastman Kodak Company, the limits were found to be 50 to 100 (Rittenhouse). Their low re sults were probably due to their method of detecting incompati bility, in which delicate optical methods were employed to detect
haze in the film.
The work on the effect of Aroclors upon the rate of burning of
cellulose acetate films, aa given in the table, leads to the following conclusions;
1. Cellulose Acetate alone burns slowly. '
2. The rate of burning, where burning takes place at all-, is accelerated by each of the substances tried.
5. While the Aroclors Increase the rat* of burning, they at the same time give a flickering uncertain flame' which
. tends to go out, that is, they tend to quench the flame.
4. Triphenyl Phosphate it an effective flameproofer, it be ing impossible to Ignite the film containing 250 of it.
5. If flexibility and lack of tendency of the film to wrinkle
or curl on drying is taken as a criterion of plasticizing
power, -the Aroclors are more effective plasticizers than '
either &1butyl phtbalate or Trlcresyl Phosphate. .
.
6. The thick film containing 25? Aroclor 125* (slightly
below the compatibility limit for thin films) was blushed.
Thia ls- in accord with the earlier observations of. the
effect of film thickness on the compatibility limit*
'
Company (756593) has found that mixtures' of decachlorodiphenyl ' and styrene are con-inflaomable and hav* a heat distortion point
20P higher than polystyrene. . (
United States Patent*o.2,227,6>7, - asigned to Leverkusen-1.<J._j . Verk, describes a composition of matter cooprlafog's realn-like. chlorinated diphenyl of aa average 'chlorine. cootent^of->bout 620 .
J* **' *
TOWOLDMONOOQ1612
r IKJiOAItTO CHEMICAL COMPART and about 7.5Jf of polyvinyl carbaxole.
10-1-44:
_ ROBBER-
` `'
' Ccopany (297400) bar* found that Aroclor 1262 la the boat plastlclxer for rubber hydrochloride. It la ccnpatlble up to 100
rubber hydrochloride, although the usual working range la 5 to 10% of Aroclor 1262 based on the weight of the chlorinated rubber. Below 50$ Aroclor no difficulty la encountered with brittleness. Aroclor tends to Increase the gloss of rubber hydrochloride films, e.g., Plioform, Pliofilm, Pllollte. Five por cent rubber hydro chloride added to Aroclor reduces the tack. . ...... - - -.
On the other hand. Company (331850) recommends the use of Aroclor 1254 with chlorinated rubber, e.g, Parlon.
QUMk 5-
rA rubber composition of reduced flammability comprlslie: P.^-TV.
Rubber
100 parts
Chlorinated rubber
35 part*
Aroclor*
:
65 parts
Sulfur
2.8 parts
Zinc Oxide
` 5 parts
Vulcanising Accelerator
1 part
C Ammonium Borate -
40 parts
Thic composition shows a flame resistance'and a notable absence
of melting around the burning material.
Aroclor 1268 is used in the manufacture of Cellular rubber of low
flammability for the aircraft Industry. ` ;..
, ,.
Company (234144) has found that 15 of Aroclor 1242 added to
Vlstlnex (polybutene) makes a de-icing coating for airplane pro
pellers that looks promising. By the addition of plasticiser
C-2V or plasticizer SC, low temperature characteristics can be
obtained.
....
..............
--
It is indicated that' Aroclor 1242 may act as a solvent for one of
the materials which la producing tack in Buna S..
.. . ...
The characteristic*, of Typa l Reoprenp compos Itloos are said to
be Improved by the addition of Aroclor 1254 increasing water
-
resistance. (Company l6947)'.V^^,r-/^^^^
-
The use of Arcc1or 5160 Is under InveatIgatiom as an extender^for Hycar OR. . ' " .. \
,.,,i ,
TOWOLDMONOOQ1613
MOJOARTO CHEMICAL COMPARE
As a plasticiser for bard rubber
Aroclor 126? baa bean used as a plasticise!* for bard rubber in
dental plates, etc., for a couple of jears*. It should be equally
useful In plasticising hard rubber for other purposes where
brittleness is undesirable.
: . r: ~'
To render lubber pemanently tacky
Aroclors 1262 and 125* ere allied Into rubber so as to make a hcnogeneous compound which has permanent tackiness or adhesion.
To flameproof rubber. Reoprene, and other synthetic rubbers
Aroclor 1269 is a hard crystalline material of high melting point.
It may be ground very fine. This finely ground Aroclor Is milled
into the rubber just as any inert filler would be. The milling
temperature is not high enough to melt this Aroclor and so there
Is no solvent action. It has been found that the Incorporation
of stifficient Aroclor 1269 in rubber prevents the spread of flame.
This is suggested especially for flameproofing rubber for use on
insulated wire.
.'
. '
...
% . THERMOSTATS
.
v
:
Aroclor 1248 is being used by several manufacturers c: thermo
stats as the expanding medium in the bulb. Aroclor has been
used in this service by one manufacturer for the last ten years.
Aroclor has proved entirely satisfactory. Every precaution must
be taken to ellminats the possibility of moisture or other for
eign matter getting into the Aroolor. The thermostat equipment
must be thoroughly cleaned before filling.
_
.*
*-
. ,e '
. * '; * '
'
Ve do not recooraend the use of Aroclor at temperatures above
6ooop (515C). * . ...
*
-.
~
-
'
TEXTILES
Company (645300): reports that Aroclors, although more expensive, exert better fIra retardant effeot than chlorinated paraffins and smaller amounts are required
Company f649900)- claimed that Aroelors 1262 and 5466"shoved a
10% increase in tensile strength when substituted for the stand
ard Jeffersonville Quartermaster Depot specified iapregnant for
POP., Uch-i.
... . V
. 41* Copper
...
.
14$ Asphalt
..... : - . 30* Paraffin Vaxr
. .. 15* Mineral Seal'
''
' ~ir r ~ ~~i ~~ 'Tiir&ggSgfc
6BRN002050
m
TOWOLDMONOOQ1614
mmXKTO CHEMICAL CCMPAHI ~
~ Xd-I-M '
Aroclor 1260 la proposed as a flameprooflug, waterproofing, mil
dewproofing agent In the produotlon of J.Q.D.*s specification 242 paullns and tentage for army use. Zzact formulation* and approval
of the Quartermaster Corps has not yet been worked out.
WOOD-
Aroclor as an Introfler for Sulfur In Wood Impregnation
It has been found desirable for sane purposes to Impregnate wood
and other fibrous materials with sulfur. However, sulfur does
not go Into these materials without difficulty. The use of 10% .
of Aroclor 4465 mixed with the sulfur acts as an introfler, caus
ing thorough penetration.
-
.
-
The Impregnation is performed as follows:
*
A mixture of 90% sulfur and 10% Aroclor 4465 Is melted and mixed
and placed In an autoclave or pressure tank with the wood or other
material to be Impregnated and held at a temperature of 125C to
140C and a pressure or 100 pounds per square Ineh. The time
necessary depends upon the kind of wood or other material being
treated. . The initial freeslng point of this mixture is 107.5C. . 1 The viscosity at 125C is reported as 27 Seconds Saybolt Universal. /
A typical impregnation of a yellow- pine 2" x 8" plank gave an increase In weight of 127% and about 100% in tensile strength.
The valuable qualities contributed by this treatment are added
strength, rigidity, resistance to moisture, to acids and to
splintering. The electrical Insulating properties are increased.
The wood Is made practically free from the effect of weather and
resists attack by insects. The treated wood is practically free
from shrinkage and swelling*.
.
Possible uses oif wood treated* In this way are:
Transmission line croesarms.
*
Tanks to resist acids, etc.
.
..
. SqulpmeftV & which swelling or splintering Is
objectionable. "- sp;r;
*
* *
. . .. -7
~
... .
; . .. .'Timbers likely to be .attacked by termites, etc. ,
_
..
--
-- -
: * Perhaps many other 'applications wBiefre the qualities .'
. . described above-are desirable; `
...7.-"-'
.
The requirement Is that the wood so treated should, stand being -v-V*
used 15 or 20 times la concrete- forms, that, it must- remain smooth, and not show annular ring or groin structure bn. the concrete..--
TOWOLDMONOOQ1615
mmueto chbmicax. cokpa** > ^ v: v ; '
where the forma are used. Plywood impregnated with a mixture
of Aroclor 2565 and 10-20* hard paraffin (melting point 60-6fiC)
would be suitable for the construction of concrete forme. Addi
tion of sulfur up to 20* of the mixture may be beneficial in
reducing the cost of impregnating material and in making the
treated wood harder. .
. ,* - , : * . . '.7 'f.r-r-1 2-"% '' v'
The reocoznended procedure' conalate of keeping the plywood sub-
merged for 30 minutes In the Aroolor-Paraffln mixture (or Aro-
clor. Paraffin, Sulfur mixture) at 80-90C,. then letting the
boards drain at about 50C and passing them between rollers to
wipe off the excess of the wax. . ... . ..... ...... -.4.
'
.
.. ` '
` "'** " v ; *- k'\. .
Plywood treated in this manner Increases in weight from 31 to 66%
and gains only 3.1 to 5.75k In weight when iamwrsed in water for
six hours. Untreated wood gain* 29% in weight when kept In water
for an equal length of time. - ; . -
--;
` *
Standard' maple wood blocks used by the shoe last Indus try ` from
~
(Company 769520) were treated with various compounds to prevent :,,...*
dimensional change from water absorption. The most effective ~
composition was found to consist of:
-
70* Aroclor 2565
20% Paraffin (hard or soft)
. 10* Sulfur *
.
. - ,v: . ,,
*
When this composition was applied under the conditions shown be-'
low the resultq indicated.were obtained:
:~
^ ...
- ----
/
--Iffeet of Soaking
<:;/-
.
in Water 2k hrs.
'>
Weight of
'
. 5T7er"
.. ,-c- t-'.-.c.i -Treatment . Gain'In Vt. imeter
' sg/sq.ln.Surface g/eq.Meter. change
1.* 60 min. at 100C.t ..--4;::.:-^:
_____
~ . ... .
30 min. cooling _ .1^ '-i: 45.36
340 ; ` 0.349
- z-rrzz. -rv~ 2. 60 mln. at lOOOC.j' -a^^-, ----- -
. - ..
. .-
30- min* eool1ng7'.7-r-r*^r'^ 42*96-
v -375rW*^.:-.' 0*349
3.- 60 min. at 100"0*j 30 min. cooling
4. 60 min. at ' 30 min. cooling'
'
,>- 49.26
...
!--W^-K-.^549 . . -
5. Vac. 30 min. at90U^ 5 min., released 10 mini?
. Maximua tolerable
TOWOLDMON00016I6
.
`i
, :
10-1-44
r NOIBAIITO CBEMICAXrTCOM?AST
Frcm another series of tests conducted on hickory fishing pole
handles it Is concluded that the best results will be obtained
using the following conditions s
r . > -
Temperature
.
Vacuum
- -'
Atmospheric pressure
Remove, drain and dry
90-100C 16-100 mm'. for 25 min.
5 min. , .
Purdue University found that Aroclor 1242 was very useful as a
base upon which to flow gelatin solutions for the production of
films, thus making it possible to eliminate mercury for this,
purpose.
-. . -
As a result of interest aroused in the Aroclors, several sugges tions have been made regarding uses which may prove of value.
1. Aroclor 1260 as an adhesive In a Joint compound for glass
building blocks. ..
#"
2. A water emulsion of Aroelor 1262 for use in leather, paper,
r textiles, rubber and casein paints.
.
3. As a protectivs coating on certain pigments to prsvent "liverlng" of paints containing resins of a high acid number. Specifically, slno oxide pigment in water emul sion of "Aquaplexj' a water emulelflable alkyd resin. -
4. A waterproofing for concrete.
*-
' \.. .
5. Aroclor 1262 or 5460 as an ingredient of molding' composi- t
tions made with such materials as ethyl cellulose, bensyl
cellulose, soy beam meal and corn protein.
.-
TOWOLDMONOOQ1617
`"
' ''#' ,':'*4 **. io-x-44
Monsanto chwical compart
-
SUOGBSTSD FORMULAS TOR MOISTUREPROOFING '__________ COMPOUNDS________ _________
Ccmpottod A
*-'
1.
96.0% Aroclor 5460 ' ,4.0% Bard Paraffin
Compound B
`.
96.0% Aroclor 4465 ' 4.0% Hard Paraffin.'- ....
* Compound C
. '. 96.0% Aroclor 5060 . 4.0% Hard Paraffin
Compound D
.
` ...... ... `. .
*
96.0% Aroclor 4065
.4,0% Hard.Paraffin......
: - - *+ .
-
-
When a relatively low softening point material is de-
aired, ve suggest those compounds using Aroclor 4465*
When a higher softening point is required, ve suggest
the compounds using Aroclor 5460. .
'. . .
Compounds C and D are black materials and are useful
vhere color is of no importance. .
.
Ve do not prepare these compounds. .
T/.'.
TOWOLDMONOOOI6I8