PROCESS specification APPLICATION OF ASBESTOS COMPOUND BY SPRAYINQ
60-01-11
General
This specification covers the application of sprayed Insulation on the Inside surfaces of steam turbine laggings for the purpose of Insulation and sound deadening.
Ma teria 1
The material used for this process is as listed below:-
W.s. Material #4057-3-
Equipment
The equipment to be used is as listed below or its equlvalent:-
Eclipse Air Bruch Co. "46" Spray Gun with Cone Nozzle and 1/4" fluid tip Eclipse #7835 Pump, 4 to 1 ratio suitable hoses for carrying 60 psi atomizing pressure and 60 psl fluid pressure.
Operations
1) Cleaning lagging 2) Application of Primer Coat
13) Application of Anchor Coating
4) Application of Second Coating 5) Application of Final Coating
It is recommended that the above operations be performed to the lagging while in the assembled condition.
(1) Cleaning Lagging
Remove all dirt, oil, grease, rust and other foreign matter from the metal surfaces to be coated. This operation to be accomplished by using mineral spirits or 6305-I, followed by wiping with a clean cloth.
Cautloni Ventilation must be provided to avoid accumulation of vapors..Refer to Safe Practice Data Sheet T-4.
(2) Application of Primer Coat
Apply one (1) coat of primer 6449 -1 to all surfaces that will be sprayed with insulation #4057-3*
600021
WESTINGHOUSE ELECTRIC CORPORATION PHILA. PA. U.SA.
<;TrAii rm/inrsM
---
----
__6_0_01111.
60-01-11
APPLICATION OF ASB.'C.TOS COMPOUND DY SPRAYING
(3) Application of Anchor Coat
Apply one coat of the compound by sorjying to cover 5 P!>-*or.lmately o of the surface, i.c., 20^ of the ba3e r.etal will "how through the insulating conpound. The- compound Is applied by holding, the spray gun approximately tlirce feet from the lagging.
The surface will appear mottled. Air dry this casting for a minimum of one (1) hour.
Note;- The anchor coat should always be insulated with compound from a barrel that has not been previously opened. A previously opened and resealed drum nay be used for later coats.
(4) Application of Second Coat
Spray on a heavy coating to a wet film thickness of 3/l6 of an inch. This is to be applied by spraying with sufficient number of passes to build up to 3/l6 of an inch and prevent any running or sagging of the compound.
Before the applied insulation has time to set up, separate the Joints where the turbine lagging is to be disassembled using a parting tool. Air dry this coat for a minimum of two (2) hours.
(5) Application of Final Coat
Spray on a final coat to increase the final film thickness to 1/4 of an inch minimum. Separate the joint3 with the use of a parting tool before the insulation has time to set up. Air dry for a minimum of 24 hours.
Caution
The operator a.hould wear an air-supply type respirator. Keep flames and sparks away from the insulation material. Refer to Safe Practice Data Sheet E-l.
The material is supplied in 30 gallon drums with clamped sealed tops. Always keep material scaled when not in use.
Order insulating conpound for coverage of 4.5 square feet per gallon.
r
j
600111 Page 2 of 2
J. W. Desmond, Mfg. Engineer L.&M.T. Erection and Test
v
600022
westinghouse. electric CORPORATION PHILA. pa. U.S.A.
STEAM DIVISION