Document jg6Y8Zy8x57rMK8r9QEZJZ30Q
+ J
N CC : Mr. E. R Coin !-*r. R.S. Weatherly Hr. Paul Logua Mr. F. R. Williams Mr. II. F. Weaver
-"y I*. F. A. Barker Mr. W. 0. Krunmrich (S) Mr. F. E, Hubbard
TRIP REPORT 214
HESTIM3H0TJSS ELECTRIC AND HANUFACTORINO COMPART . East Pittsburgh, Pennsylvania October 14-15, 1943 *
A meeting was held with men representing the Research, Engineering, and Purchasing Departments of Westinghouse at whioh revisions of the specifications for Aroclor 1254 (Inerteen 6935-1) were discussed in detail and oertain agreements were reached; and a later meeting was held with the Research group (Insulation Division) corresponding to F,, U, Clark's group at General Electrio Company at whioh the question of air-cooled transformers vs. Ivertoen-filled transformers was disoussed and interest was aroused in oertain of our new products.
In the following are notes, on the two meetings. These are given in con siderable detail, pertly so as to have a reasonably complete record of what went on and also because these meetings were the first direct oontaot between Anniston Research and Westinghouse technical men in something over ten years.
MEETING OF OCTOBER 14
Present: '
-
-
`
Dr. R, N. Evans, Insulation Division of Research Laboratory
Dr. L. J. Berberioh, Insulation Division of Research Laboratory
Mr. P, E. Demmler, Engineer, Feeder Department
Mr. R. E, Merbury, Engineer Switoh-gear Department. (Circuit Breakers
and Protective devises)
Mr, C. V. Fields, Engineer Switoh-gear Department (Circuit breakers
and Protective Devioes)
Mr. Gilbert Remley, Purchasing Department
Dr. L. Jenkins, Monsanto
Messrs. Marbury and Fields were introduced as interested in design and
manufacture of capacitors, although their department and activity were given in
the directory as shown above. '
i
.
-
The meeting was arranged by Mr. H. H. Hartness, of the Purchasing Department
of Westinghouse, through Mr. Weatherly.
.'
*.
.'
In preparation for tank oar' shiprfsntB of Aroclor 1254 (capacitor Insrteen), Westinghouse is Installing a 15,000 gallon storage tank end a fuller's earth treater and filter for the individual batches (about 150 gallons each) to be with drawn from the storage and delivered to the capaoiter impregnating units.
Their existing treating and handling equipment has been satisfactory for handling Aroclor 1254 received in drums. It is interesting to note that they "sucked," rather than pumped, the Aroclor from the drums and through a tall bed" of fuller's earth to their oharging tanka for the capacitor treaters.
DSW 331019
STLCOPCB4077663
2-- Trip Report 214
They are planning to draw the Aroolpr from the tank oar into the storage
tank by vaouurn and to hold the Aroolor at a temperature above ordinary
temperatures in the storage tank and at a vaouurn of around 26" of meroury0
The disign oalls for a oatoh tank to collect any condensate between the stoeage
tank and the vacuum pump.
',
>
The plan was to hold the .Aroolor while in storage at 85*C. They expressed
concern about fractional evaporation of the Aroolor that might affeot the
properties of the product. Later Dr. Berberioh remarked that he had oarried
out tests on this point and had found that a little evaporation improved
'
(decreased) the power faotor whioh was regarded as the most important property.
The possible change (Increase) in viscosity, specifio gravity and dielectric
constant as a result of evaporation in storage was regarded as of less importance.
I suggested they drop the temperature somewhat below 85*0 so as to avoid
excessive fractional evaporation. Marbury agreed that they would try 50#0
and even go lower provided their transfer system would then still handle the
material.
'
They anticipate consumption of two tank oars of Aroclor 1254 per month0 If the inventory in the storage tank is maintained at from one-half full to full, this will mean a relatively slow turnover in the hot storage. They particularly asked whether I had any reason to believe that the hot storage would be harmful to the Aroolor in any respect other than possible fractional evaporation of the Aroolor. I know of no harmful effect. If any iron is picked up it would presumably be removed by their fuller#e earth treatment
between the storage tank and the oapaoiter treaters.
The primary object of the meeting was revision of specifications whioh they
thought desirable for tank car shipment. Actually, the real reason for their
renewed interest was presumably the new arrangement (not mentioned during the
meeting) whereby we will sell dlreot to Westinghouse rather than through the
General Eleotrio Co. Marbury presented a detailed graph of the data as given
in Monsanto's test certificates for shipments of Aroclor 1254 from October
i37 to February 1942 and pointed out that apparently our own data showed the
shipments frequently fell outside our specifications. Specifically the graf^
indicated the following:
.
Specific gravity always within specifications.
'
Pour point within specifications, exoept certificate of November 14,
1940. Yisoosity within specifications only 10 times out of 25 shipments (this point was cleared up in the disoussion the next day with
Dr. Evans).
Color OK Acid number OK Heat loss OK
, -
DSW 331020
r
STLCOPCB4077664
l 3--Trip Report 214
.Distillation range completely within, specifications only twice out of
25 shipments '
Dioleotrio constant within specifications only 11 times out of 2 ship
ments.
.
Resistivity always within specification but quite variable (100
to 1500 i l69 ohms/om.fcy, *
.
They were seriously concerned as to whether we would supply then a uniform
produot within specification although they had to admit that the product had been satisfactory in aotual service and consequently the apparent deviatlons in properties of the produot were not serious.
They were also concerned that they be given as good a grade of Aroclor 1254 as their ohlef competitor and I ensured then that the same material has been and will be supplied to themes we supply to other eleotrio companies.
I told them that I did not usually see any of tpe test certificates and
therefore was not in a position to disouss the variations shown on their chart,
but I would check up on this question and write them. I pointed out that some
of the test data that they complained about were incompatible with other data
oh the same sample . For example, the certificate of November 14, 1940 showed
a high pour point (one point or 2*0 above the iraximum apeoifi oat ion) and yet the
visoosity and specific gravity ware normal, which would indioate an error in
the determination or in copying the data. There were four errors in the chart
in designating absolssas and ordinates (which, however, did not change the
conclusions), and I judged that it had been very hurriedly drawn up by Mr.
Marbury for
................
the
me, e, t,in, g, .
*
Specification Revision
. *
'
. ' if
.
Copies of Westinghouse predent specifications for Jnsrteen 6935-1 (Aroclor
1254) and of proposed new spooifioations were presented end discussed in detail.
With the group as. large as It wap, it was impossible to reach definite agree
ment on the various items and it was agreed that I would take the. various
suggestions, go over the proposed specifications, check.with >ur (derating and
Sales Departments, and send them our revision for their consi'eracion. Correspon
dence should be directed to Dr. Evans with copies to Dr. C. F. Hill (Evan's
superior), Mr. Marbury, and Mr. Remley,
.'
'
Actually few Changes in specification will be necessary in order to satisfy We stinghouse. Dr. Evans said they did not want to place unduly strict specification limits on the produot which were not warranted and which would work a hardship on us.
The data shown by their graph, described above, must be cheoked to ascertain the apparently wide discrepancies between our test results in certain instances
and our specifications, particularly with respeot to distillation range and dielectric constant. The matter of viscosity was cleared up in a discussion with Dr, Evans the next morning and it was agreed that the specification would be changed from the Gr. E. value of 45 to 49 seconds to 44.5 to 47.5 seconds which is the range obtained with our calibrated viscosimeter on normal Ardor 1254. All shipments to Westinghouse since 1937 have oomformed to the latter
llmitSo
DSW 331021
STLCOPCB4077665
4--Trip Report 214
la general Westinghouse would like to have the specifications narrowed
up although again they expressly stated they.do not want to place any undue
hardship upon Us.
_
Following Qre notes on their suggestions oh speoifio items,which are numbered below as in their proposed new specification sheet:
1, Description, They want a more aoourate description than
"Pentaohlor-Di-Phenyl - a j&e yellow, viscous liquid at room temperature."
Suggestion*. A mixture of chlorinated diphenyls having an average chlorine
oontent approximately that of Pentaohlor-dlphenyl and possessing the
ohemloal and physioal properties described in sections 3 to 14 inclusive
helow,
'
2, Seotion stating that no ohango in quality shall be made without approval - no comments
3, Aoidity. Dr. Evans suggested that the limit of 0,01 be lowered.
According to their graph the a old numbers of all shipments since October
1937 have been 0,007 or lower and since November 1939 have been below
0.005.
Dr. Evans pointed out that the acid number data are not comparable with the figures for free ohlorldes assuming both are due to HC1. An acid number of 0.01 is equivalent to free ohlorldes of 8.88 ppm. Since our free chlorides do not run over 0,15 ppm, there must be some aoid other than HG1 in the Aroolor or, alternatively, the extraction method for free chlorides oatohes only a very small portion of the H01 or aoid chlorides present, I believe that the latter has been disproved at St. Louis by successive extraction tests.
We have been aware of these facts for a long time, but are dealing with suoh minute quantitfea of impurities (0.01 acid number is equivalent to 0,001% H01 or 0*01% of an acid monohydroxy-pentaahlorodiphenyl) that chemical methods of identifying the acid or acids present is at least difficult.
Dr Evans pointed out that ferric chloride added to the Aroclor in an amount equivalent to 0,15 ppm of chlorides imparts a very high dielectric
loss to the Aroolor. Consequently, he argued that the chlorides cannot be
present as ferric chloride with whioh I agreed upon the bases of the other evidence,
I pointed out to Dr. Evans that Aroolor 1254 with sn aoid number less than 0.01 and free-Chlorides test not over 0.15 ppm had been proved satis factory for capaoitors; that the specification limits whatever their real significance as to impurities, had been found quite satisfactory indications
SW 331022
(r
STLCOPCB4077666
5---Trip Report 14
of useable rAroolor from several years of experience.
He understood this point but emphasized the faot that he oould make
up an Aroclor by adding nlnute amounts of, say, ferrio chloride that would
pass both the acid number and free ohlorides tests and yet oould be quite
unsatisfactory as q dielectric. I agreed that this was true but pointed
out that other tests (specifically resistivity, power factor or dieleotrio
loss) would catch such a situation.
*
I agreed to disouss with Operating Departments of Anniston and Plant B a possible lowering of the specification limit on acid number. However, I do not recommend a change in this specification.
4. Ohlorides. Discussed above. The test method and specification
limit was worked in cooperation with 0. E. Co., and .I would not reoomnerfl
a ohange from our present "0.15 ppm max." which should replaoe Westing-
house's specification of "none."
-
At Dr. Evans Request, I agreed to.aske tfc .Analytical Laboratory to
test the pH of the water extract for a series of-shipments and reoort the
results to him.
. '
5o Distillation Range. Discrepancies between our test results and
specifications as shown on Westinghouse's graph should be oheoked up.
Actually the 1 per Qent point, nobnow included in the specification might
well be added.
.
6. Condition - No oomment.
7. Speoifio Gravity - No oomment. ,
8. Viscosity. Since Westinghouse do not run viscosity themselves and plan to continue to rely upon our test results the specification should be amended to the range (44.5 to 47.5 seconds) that we get on our calibrated viscosimeter.
9. Color. This was not disoussed but should be amended to read on the AEHA scale and probably 150 AEHA max. to conform with the tentative specification of G. E. Oo.
10. Pour Point. No comments '
^ 11. Eleotrioal Resistivity. No ohange in items (a) and (b) whioh con form to G. E'a standard specifications. Cheok as to whether voltage we use oonforma. Item (o) states that samples used for electrical resistivity
DSW 331023
STLCOPCB4077667
6--Trip Report 214
tests "may be treated by contact with 2XF Florez B absorbent or approve#
equivalent ...
This should be omitted or made mandatory, preferably
omitted. If mandatory, the exact treating procedure should be opacified.
22. Dielectric Constant. Specification limits should not be changed but the reason why half of the shipments as shown an the Westinghouse graph fell outside specifications should be checked up und Westinghouse assured of future conformance with specifications.
13. Power Faotor. I told them that we do not usually determine power factor and they did not Insist on our doing so.
Even though we are not likely to be called upon to determine power factor, the specification should be inoluded. The exact procedure for treating with clay prior to the test must be specified and the frequency (they give 60 cycles) in the actual test &ust be agreed upon,
14. Heating loss. Specification is 0.4% max. Since no shipment ! (according to their grapi) has shown greater than 0.01 since October 1937, I
see no reason against aooeding to their suggestion to lower the limit. They are interested in this Item because.of their plans for hot storage under vacuum. The &ualytioai laboratory should have a standard rotating shelf oven for their test, -
15. Packing - No comments.
16. Drums - No comments.
17. Bung - No comments.
18. Marking - No comments.
,
19. Marking for Tank Cars - No comments.
20. Inspection. This section provides that a "certified test report be supplied with each shipment. By this they meant a certificate sworn to before a notary. I told them we could have each report notarized if they insistp^but I thought it unnecessary. I recommend we omit the work "certified" in our revision to be sent to Westinghouss,
The list of tests to be included in our test report should be amended (a) by changing color from HPA to APHA scale and (b) omit power factor
The list of tests to be inoluded in our test report will then be as follows:
Specific Gravity at 668C/l5.5*C Color (APHA.) Condition Acidity
DSW 331024
,r' (
STLCOPCB4077668
7--Trip Report 214
)
Free Chlorides
Pour Point Viscosity at 98,9*0 Distillation Range
1# point (?)
90$ point
Dielectric Constant
Resistivity
,
210 Shipment, This section provides that shipment may be made with out approval provided our tests show the product to be within all specifica tions, The test report is forwarded to Westinghouse at the time of shipment'
Incase the product fails to meet any speoifioation test, the test report is forwarded to Westinghouse and shipment is withheld until approval is given,
I see no need for revision,
.
22o Rejection clause,
. Westinghouse reserves the right to reject ... material that does not conform to the above specification in every particular . , ,
It should be mentioned that, while Westinghouse will depend upon us for tests of the Aroolor before sh^nent, they plan to sample the tank oar before dumping and test for resistivity and power factor.
Please note that no suggestion was made by Westinghouse to include a specification for water content. Even though this test is not included in the Westinghouse speoifioation, I recommend it be run by us as a plant oontrol test for all lots of Aroclor 1254 to be sent to Westinghouse and as protection to ourselves, ,
Contamination of Tank Cars
Westinghouse will attach breathers to the tank cars so as to avoid entranoe of moisture during unloading, .
They particularly asked about cleanliness of returned oars as received by
us from other customers, particularly whether we drained any heel and cleaned the
oar, I told them that we oarefully inspected the oar
if it had an appreciable
heel (we usually find as much as 50 gallons) this heel is sampled and tested. If
okay, the oar is then filled. If not or if the oar is not perfectly clean, it
is thoroughly cleaned before filling.
DSW 331025
STLCOPCB4077669
8--Trip iteport 214
Complaints:
Ur, Uarbury Mentioned our use of a different type of drun in a ehipnent of about Decaaber 1941. This drum had a crinped-on head of a type that would not stand a severe blow without parting at tho crimp. He claimed so w 25 drums had been received with sufficiently large holes to admit moisture to the Aroolor. I found that a complaint had been rade through the proper channels
and dropped the matter. .
, Utr. Marbury also claimed that shipments in 1942 have shown a decided increase in accumulations of Aroolor in their vacuum lines. They impregnate their paper-spaced capacitors with a vacuum of around 260 to 300 microns. They did not specify temperature. 1 suggested we could check up on any change in the Aroclor that might have oaused this trouble by comparing evaporation loss tests and distillation temperatures at and 105*3, They did not have the data available. The follwolng day. Dr. Berberlch told be he thought that there had been no change in the Aroclor and that the production men had Just begun to notioe the accumulations in their vacuum lines which had always occurred. I
am inclined to believe Dr. Berberlch.
The complaint was made by Hr. Marbury that beginning in 1942 they had
had trouble with Increased dielectric loss. This had begun in January and was
at a peak in April 1942. The situation has their paper Bpacer that was in part
responsible but, over and above that, he felt there had been some change in the
Aroclor that was partly the cause for the high dielectric loss of condensers
made during this period, I offered to try to get sufficient samples of Aro-
clors made in 1941 and during the bad period (April) of 1942 so that exact
electrical comparisons oould be made. He did not want me to send them now.
The following day, the natter was discussed with Dr. Hill who felt that the
trouble was due to other factors mainly their paper, and not due to the
Aroclor.
...
If I recall oorrectly, Clark of O. ran into similar troubles some 5 years
ago and actually had to aake a study of paper manufacture and finally tell the , manufacturers how to improve their paper.
Special Tests and Test Methoda
.
Westinghouse uses a continuous resistivity tester which is set direotly in their Aroolor pipe lines. Marbury said it was very simple--only a cell like our resistivity oell set in the line with axis parallel to the flow of the Aroolor and connected to the usual testing equipment. He suggested we put it in our line to storage tank or tank oar.
Dr. Evans asked for our data on resistivity vs. moisture content of Aroolor 1254a This will have to be obtained from St. Louis
Dr. Evans suggested we look into the A.S.T.M. method for free mineral aoidity
as a possible procedure for distinguishing between HOI and organio acids in our Aroolor. He will send us further information.
DSW 331026
STLCOPCB4077670
{) 9--Trip Report 14
Dr. Evans asked about our opinion of the cloud point nethod for deter-'
mining moisture contents ^ told him we had long ago abandoned it in favor of the Fischer method and he was entirely in agreement. However, he remarked that they had a method whioh he regarded as more satisfactory than even the Fisher method but did not give it to us.
Chlorine Supply
Marbury particularly asked whether I knew any reason why they should be concerned about supply of chlorine for their increased requirements of Aroolor 1254* I told them that nothing that I knew indicated a shortage at present. There is a rumor of a huge new war demand tor chlorine that may break at any time, but I have taken this rumor with a grain of salt and thought it unwise to mention it to the&*
Crystals in Aroolor 1254
Dr. Evans told me that in some of their Aroolor 1254 pipe lines there had
been found crystals containing copper, iron, and an organic material that could
be extracted with benzene and that crystallized before evaporation of the benzene.
A sample was obtained,
-
Power Factor
Dr. Berberich was particularly interested in F. M. Clark* s curve (U. S,
Patent
} showing a minimum power faotor at the pentachlor stage in the
Aroolor series. Neither he nor Dr, Hill (idiom I saw the followihg day) believed
the curve correct and asked for fresh samples of Aroclors with higher and lower
chlorine contents so as to check the data. Two- quart samples have been sent
of Aroolors 1242, 1243, and 1260.
Treating Olay
Westinghouse uses a "hard burned** fuller's earth which had been treated to
900aF during the calcining prooess. It is obtained as 100 mesh material from
the Florid ia Co. and is designated as XXF Florex B adsorbent. Before use it is
heated to> 225*-250C for 24 hours and is then stored in a room at 100*0 until
needed. .
,
They have found it much lore effective than Attapulgus earth, particularly in lowering the power faotor of the Aroolor. ...
We will obtain samples.
Mr. Marbury asked for a oopy of the Aroolor booklet. I left my copy with
Dr. Evans.
.,
DSW 331027 STLCOPCB4077671
10--Trip Report 214
MEETING OF OCTOBER 15*
The entire afternoon of October 14 was taken up with discussions of speci fications and related aubjeots. I went back the following morning on invitation of Dr. C. F. Hillt iiwnBgqj. of the Insulation Division of Researoh, who is an old friend. Dr. Berberioh and Dr. Evans were present part of the morning.
Dr. Berberioh gave some details of the.evaporation tests he had mentioned
the day before* Actually there were distillation tests using an A. S. T. M.
distillation flask without fraotuating nolumn and at 1 mm pressure. Weights
were not given.
'
Distilling Range Power Factor LightTransmission 01- Per Cent
`(Peroent)
Original Aroclor 1254
-
.13
not given
54.9
Fraction 1
100*-134*C
.20
79.2#
52.5
Fraction 2
. 134*-140*0
.09
79.0
53.6
Fraction 3
140*-147*C
.08
77.9
55.4
Residue
J.3
50,5
58.0
The test showed that removal of a low boiling fraction reduced (improved) the power faotor but it seems to me a much more direct and practical test oould
be devised for determining the effeot of hot vacuum storage on power faotor of Aroclor 1254.
Dr. Hill remembered that the lower Aroolors are not as stable electrioally as Aroclor 1254.
Dr. Berber!ch has observed that the color of Aroclor 1254 is removed*from some samples and not from others and was particularly interested in just what the color is due to. This is a point on whioh we have little information exoept that it is not due to ferric ohloride (whioh imparts a similar color to white Aroolor) and is probably due to minute traoes of highly colored organic compounds. I told them a spectrographio study is now being made of Aroclor 1254. (It should be noted that the German equivalent of Aroclor 1254 - Clophen - is water white)o
I was impressed by the difference in attitude of Hill's group as oompa red to Clark's group at G. E. Co. The former is inclined twward the academic research approaoh with a yen for detail and a desire to know the reason why for each new observation while Clark is more the practical application man who is satisfied once he has obtained the desired result.
There is a real rivalry between the fcwo laboratories. In spite of the faot that Westlnghouse and General Electric have had a aross-lioensing agreement for many years each wants to come out first with a new development and each is in clined to minimize the new things developed by the others.
v
*By their fuller's earth treatment
/ (
DSW 331028
\ STLCOPCB4077672
4
11-Trip Report 814
I avoided mention of 0. E. Co., but Dr. Hill insisted on bringing up the subjeot, telling me onoe that on these occasions when Westinghouse had beat G. E. to a new development, Clark would'usually work for a period of time to get something better and then often had to give up and take a license from Nestinghouse after all. He said laughingly that sometimes the tables were turned.
At another time, he said that Swann had offered Nestinghouse the Aroolor
development before he had offered it to G. E. Co., but Weatinghouse had not seen fit to follow it up at that time, in part because Swann had wanted Weatinghouse to put capital into it. This does not seem to me entirely accurate.
Air-Cooled Transformers
r.
F. M. Clark of G. E. Co. has mentioned on several occasions that Westinghouse wee pushing air-cooled or nitrogen-filled transformers in place of Aroolorfilled transformers. Clark has insisted that Weatinghouse are off on the wrong track.
I asked Hill what they were doing in air-cooled transformers. He said they
were pushing them and were selling quantities for use on shipboard and for use-1
in factories where it was not convenient to plaoe the transformer in a^ fire-proof
housing. I picked this up, saying that I understood the TJnderwriters^Laboratories
had approved Ifbrteen-fllled transformers for use in any location without a
fire-proof housing. He did not direotly answer this comment but said that the '
Navy claims that any type of liquid-filled transformer is dangerous on shipboard.
If the transformer is smashed in action any liquid, even non-flammable Imerteen,
is a nuidance and even may be a real hazard.
He said he did not regard ivprteen -filled transformers as being safe even
in factories or other indoor locations unless enclosed in a fire-proof housing.
He oited the case of one such transformer:: located in an underground chamber not
closed off from the basement of a building in New York
whioh had exploded
due to a short within the transformer and had spread hot iVterteen and fumes into
the basement.
I expressed surprise that an Iverteen-fllled transformer would explode at all (in'view of G. E. tests on this point--which I did not mention), but he insisted this may ooour as a result of a bad arc within the case and would give rise to poisonous gases. I remarked that careful tests (by the Underwriters1 Laboratories) had shown no highly toxic gas (phosgene) is formed by action of an arc on Aroolor. He admitted that night be true bjrt HC1 gas le formed, which ie true. (G. E. Co. at one time talked of including an HC1 absorber in the trans former. I do not know whetter it is installed in'current models)
I know that G. E. Oo. have very carefully investigated the hazards In oonneotion with Pyranol-filled transformers and I believe they are currently advertising the safety feature when suoh transformers are located adjacent to machines in .factories,' emphasizing that no protective housing need be employed. I plan to ask Clark when I next see him whether they have ever had any accidets with a Pyranol-filled transformer. The explosion referred to by Hill might have been with their old Imerteen formulation which contained chlorinated toluene in
addition to the Aroolor--T.C.B. used by G. E. Co.
DSW 331029
STLCOPCB4077673
12--Trip Report 214
At present, Westinghouse can build air-cooled transformers for yoltages
up to only 13.8 kilovolts. These transformers must pass a test at 39 kilovolts
but are considered safe for use only up to 13.8 kv. The reason for the limit
is the relatively low dielectric strength of air as compared to oil or Iverteen.
My Impression had been that their transformers were sealed in a dry nitrogen
atmosphere but the photographs did not so indicate and they did not offer any
enlightening comments when I asked about nitrogen-filled transformers.
..
Dr. Hill remarked that a. E. Co. are now building air-cooled transformers--
which was a surprise to ms.
-
Santowaxes and HB-40'
-
'. .
Santowaxes were discussed in considerable detail. There was no place where they saw they would fit for the moment, but Dr. Berberioh asked for samples an will try ideas as they ocour to him. Thessamples have been sent.
Dr. Hill was interested in HB-40 and particularly asked about its resistance to oxidation. A sample has been sent for his examination. He remarked that oxidation tests might be run by Dr. Balabaugh of M.I.T. who has been running such tests for a group of eleotric-equipment manufacturers. He would not promise, but I believe he will make the arrangements.
Complete data sheets on Santowaxes and HB-40 will sent to Dr. Hill.
Aroolor 5442
`I
I told Dr; Hill that Aroolor 5442 has the highest dielectric constant of any in the 5400 serieB and is comparable with Aroolor 1242 but of much lower vapor pressure and higher pour point. He was interested in a sample which will, be sent.
Vinyl Terphenyl
.
While we Were discussing Santos axes, Dr. Evans asked whether we had made
vinyl'.terphenyl (diphenyl styrene). I told him this was in our program but we
had not yet made it. Dr. Hill then raised the question of Springfidd's Styramic (about which I claimed no specific knowledge). He said if this material oould
be raised in softening point to 125*0, they would be much interested in it.
-'
'
'*
'
At lunch with Dr. Hill and Dr. Berberioh, Dr. Hill brought the subjeot up
again. He said they had made vinyl diphenyl (phenyl styrene) and had copoly merized it with styrene in an effort to raise the softening point of the polystyrene. (This .is what Springfield plans to do. They have asked us to make vinyl diphenyl
for this puroose) The polystyrene is of great interest to them as a low-loss dieleotrio but has too low a softening point. The vinyl diphenyl raised the
softening ooint to about 92*0 (from about 82*0 for their polystyrene) but this
was not enough and further it rendered the plastic too brittle. If plasticizers
were added, the brittleness could be overcome, but the softening point was lowered.
I suggested the oopolymerization of a very small amount of butadiene with the styrene-vinyl diphinyl mixture with the idea that this might overcome the brittleness without appreciably lowering the softening point.
DSW 331030
(
STLCOPCB4077674
15--Trip Report 14
)
Later, In Dayton, this me discussed with Dr. Thomas. He is to supply speoial samples of certain styrene copolymers that I will submit to Dr. Hill.
Dr. Hill had been interested in vinyl earbazole which they could polymerize to give a plastio with 150*C softening point. However the produot was much too brittle. I suggested they try HB-40 as a plasticizer.
Rust Proofing
I took the liberty of asking Dr. Hill whether they were interested in a temporary rustproofing procedure for steel which we had worked out by us and whioh left no oil or grease on the surfaoe of the metal. He knew of no need but will keep it in mind. He mentioned Hr. H. D, Holler of the Chemical end Metallurgical Division of the Researoh Laboratory as the man to contact on this, but I did not have an opportunity to do so.
AB 10-22-42
R. L. Jenkins
DSW 331031
STLCOPCB4077675