Document gaMMnwJ0VkJYqrM0ZEmQBpE7L

uqnirfVj.ru me :ONOLlTE DIVISION W. R. GRACE S. CO. RESEARCH LABORATORY f(W|R0< HI - preliminary study of exclusion of ASBESTOS FIBER FROM MONO-KOTE, MX-3 November 1, 1965 Test Report No. 1231 Laboratory Data Book No. 81, pages 66, 69, 82 and 88 Work done by* R. J. Bragg, J. Wilson, w. r. payment Work requested by* E. L. Perrine Purpose of Test* This investigation has been made to provide a base reference point for planned additional efforts to de crease the cost of Mono-Kote. This goal was formally expressed at the Vermiculite Institute Plaster Coonittee meeting on October 27, 1965. Abstract* The exclusion of asbestos fiber from our Mono-Kote mk-3 formulation results in a product, which when compared with Mono-Kote, has the following properties* a) 20.8% higher dry bulk density b) 5.2% higher cured density c) 10.0% shorter set time d) 17.8% lower water requirement e) 10.3% lower raw materials cost for producer f) 5.2% higher raw materials cost for consumer To express it a bit differently, we could save $.09 per bag in manufacturing costs by eliminating asbestos. The customer would lose $.10 per bag in reduced yield (i.e. 9 $2.00 per bag selling price). It was noted that this product provided a 6.3% shorter fire endurance time than regular Mono-Kote, but re-tests may show this to be within the range of experimental error. It is sensed that seme means should be taken to lower the density of such a mix as herein discussed: perhaps bv use of the new p-16 No. 4 aggregate, more aggregate and/or more efficient air-entrain ment mechanisms. !> teat Report So. 1231 2 Procedures TVo batches of Mono-Rote were blended on 7-6-65 at Travel ere Rest, 3. C. Mix So. 61-66 is the control using the regular MK-3 formula. Mix So. 81-69 is identical with the exception that no asbeetoe fiber was used. These batches were wet mixed and applied on 7-15-65 by the author. Mixing was cone in a 6 cu. ft. mortar type mixer and. application was with the electrically driven PCC Tri Coater with SO ft. of 2* cia.s 15 ft. of IV dia* hose and 1/2* dia. orifice. Atomizing pressure was constant, at 18 peig, for both batchas. Sn addition to small samples ratalned for dry density determination, each material was applied to a 4* x 4* panel of Robertson Section 3 steel deck for subsequent fire testing. Thiekness of application was 1/2* following the contour of the fluted deck specimen. After about 1% months of curing (natural drying) thesa panels were fire tested on our pilot fire test furnace. Sand loading was usad to simulata the normal high density concrete, in order to compress time. Patat MR-3 Control (Mix 81-66) MR-3 without Fiber (Mix ei-69) Bo. 3 Domestic Vezmiculite 6 e.f. 7M Asbestos Gypsum cuponal WA Cry Total Weight 35.3 lbs. 17.7 lbs. 76.3 lbs. 60.0 cram 129.Tibs" 76.3 lbs. 60.0 cram ill.3 lbs. Dry Bulk Oansity Set time, hand mixed 20.2 pcf 4.1 hours 24.4 pef 3.7 hours Mix & Yield Data Lbs. material charged Water requirement Mixer density Morris density 75 lbs 125 lbs. 56.6 pcf 63.4 pcf 108.0 lbs 148.0 lbs 62.2 pcf 63.7 pcf Cu. Ft. per SO lbs. Bd. Ft. per 50 lbs. 2.10 25.2 1.86 22.3 Lbs. water per lb. of material % water reduction 1.667 1.370 17.8 Dry density of cured product Specimen Frame Mo. Pilot Fire Test Mo. Cure time Elapsed time to failure (minutes) 26.8 pcf 28 14 41 days 211 26.2 pef 31 17 56 days 189 25108229 fast Report So, 1231 Cata: 11 coat Analyses RMC/ Pound So, 3 Domestic Vecmiculite 3'.0236 7 M Aabeatoa .0290 Gypsum .0110 Duponal ma Dry .4800 Total Coat (RMC) Batch Weight, lbs. RMC/lb RMC/50 lb. unit Be'. Pt./SO lb. unit RMC/Bd. Pt. 3 fornula Costa MK-3 MJC-3 Control Without Piber Ofix 81-66) (Mix 81-69) $.833 .513 *839 .063 n.246 $.833 .000 .839 .063 Ji.Ws 129.3 9.0174.* 9; 870 2S.2 9*0345 111.3 $.0156 $.78 22.3 $.0350 Re*3>ectfully submitted. Manager Slcokie Laboratory RJB:ej 23108230 uqn>rfu:.rTmc ^ONOLITE DIVISION W. R. GRACE & CO. RESEARCH LABORATORY miKMSUI XOuC U.LIHOH rcuE**oc in - it-mi PRELIMINARY STUDY OF EXCLUSION OF ASBESTOS FIBER FROM MONO-NOTE, MK-3 November 1, 1965 Test Report No. 1231 Laboratory Data Book No. 81, pages 66, 69, 82 and 88 Work done by* R. J. Bragg, J. Wilson, w. R. payment Work requested by: E. L. Perrine Purpose of Testi This investigation has been made to provide a base reference point for planned additional efforts to de crease the cost of ftono-Kote. This goal was formally expressed at the Vermiculite Institute Plaster Convoittee meeting on October 27, 1965. Abstract; The exclusion of asbestos fiber from pur Mono-Kote MK-3 formulation results in a product, which when compared with Mono-Note, has the following properties: a) 20.8% higher dry bulk density b) 5.2% higher cured density c) 10.0% shorter set time d) 17.8% lower water requirement e) 10.3% lower raw materials cost for producer f) 5.2% higher raw materials cost for consumer To express it a bit differently, we could save $.09 per bag in manufacturing costs by eliminating asbestos. The customer would lose $.10 per bag in reduced yield (i.e. @ $2.00 per bag selling price). It was noted that this product provided a 6.3% shorter fire endurance time than regular Mono-Kote, but re-tests may show this to be within the range of experimental error. It is sensed that some means should be taken to lower the density of such a mix as herein discussed.- perhaps bv use of the new p-16 No. 4 aggregate, more aggregate and/or more efficient air-entrain ment mechanisms. Teat Report Ho. 1231 2 Procedure* Two batches of Mono-Kate were blended on 7-6-65 at Travelers Rest, S. C. Mix So, 01-66 Is the control using the regular MK-3 formula. Mix No. 81-69 la identical with the exception that no asbestos fiber was used. These batches were wet mixed and applied on 7-15-65 by the author. Mixing was cone in a 6 cu. ft. mortar type mixer and. application was with the electrically driven PEC Tri Coater with 50 ft. of 2* dia.j 15 ft. of 1%" dia* hose and 1/2" dia. orifice. Atomizing pressure was constant, at 18 psig, for both batches. In addition to small samples retained for dry density determination, each material was applied to a 4* x 4* panel of Robertson Section 3 steel deck for subsequent fire testing. Thickness of application was 1/2" following the contour of the fluted deck specimen. After about 1% ninths of curing (natural drying) these panels were fire tested on our pilot fire test furnace. Sand loading was used to simulate the normal high density concrete, in order to compress time. Patat MK-3 control (Mix 81-66) MK-3 without Piber (Mix ei-69) Bo. 3 Domestic Vermiculite 6 e.f. 7M Asbestos Gypsum cuponal WA Dry Total Weight 35.3 lbs. 17.7 lbs. 76.3 lbs. 60.0 cram 129.3 lbs 35.0 lbs 76.3 lbs. 60.0 cram JUL1.3 lba. Dry Bulk Density Set time, hand mixed 20.2 pef 4.1 houri 24.4 pcf 3.7 hours Mix & Yield Data Lba. material charged Water requirement Mixer density Nozzle density 75 lbs 125 lbs. S6.6 pcf 63.4 pcf 108.0 lbs 148.0 lbs 62.2 pcf 63.7 pcf Cu. Ft. per 50 lbs. Bd. Ft. per SO lbs. 2.10 25.2 1.86 22.3 Lbs. water per lb. of material % water reduction 1.667 1.370 17.8 Dry density of cured produet Specimen Frame No. Pilot Fire Test NO. Cure time Elapsed time to failure (minutes) 26.8 pcf 28 14 41 days 211 28.2 pcf 31 17 56 days 189 23108229 Test Report Ho. 1231 cats: Cost Analyses RMC/ Pound Ho. 3 Domestic Vermiculite $.0236 7 M Asbestos .0290 Gypsum .0110 Duponal Ma Dry .4800 Total Coat (RMC) Batch Weight, lbs. RMC/lb RMC/50 lb. unit Be'. Ft./SO lb. unit RMC/Bd. Ft. 3 Formula Costs MK-3 ~ Mfc-3 Control Without Fiber (fjlx 81*66) (Mix 81-69) $.833 .513 .839 .063 $2,248 $.833 .000 .839 .063 Sl.Ws" 129.3 $.0174.* $.870 25.2 $.0345 111.3 $.0156 $.78 22.3 $.0350 Respectfully submitted. Manager Skokie Laboratory RJB:ej 23108230