Research & Development Department P.0. Box 579* Niagara Falls, N.Y. July 10, 1968
MEMORANDUM
Date;
July 10, 1968
Notebook No.: 2310
TO: Dr. S. Chvastiak
FROM:
E. J. Markievicz
SUBJECT: Polyox WSRN-10 and Tergitol TP-9 Treated S-G200 for Drilling Fluid Application
Since both Polyox WSRN-10 and Tergitol TP-9 treated asbestos exhibited such good dry bulk values upon opening, samples of S-G200 were treated vith 1 and 10 parts per hundred of both chemicals. These products were both treated in a laboratory Waring Blendor at 2% solids, baroid filtered at 80 psig, dried, and slurried vith the multi-mixer for 5 and 10 minutes. Readings were taken with both a Farm 35 model viscometer at600 and 300RPM andanLVT Brookfield viscometer vith T-Bar and helipath at 0.3, 0.6,1.5,3.0, 6.0, and 12.0 RPM.
Essentially their application vas to find an easier vet opening drilling fluid additive. From the data attached, obviously the polyox treated asbestos opens no better than untreated asbestos. No testing vas done on the Tergitol TP-9 treated asbestos since excessive frothing, even at the lov loading, didn't allov any high shear mixing. The slurry foamed right out of the multi-mixer cup.
Possibly high-purity polyox treated asbestos may vet open better than untreated high-purity, but this von't be checked unless you so desire.
EJM: Jai
/j. Markievicz
X
A)707S
J.
^ersJ. AA'
A
* ....
DISTRIBUTION
J. A. Riddle
L F. Crow 0
R. O. Marsten Q
W.E.Hclsapple
A. A. Andrade Q
G. C. Brice
Shifter*
J. L. Myers
K. A. Wood
D. S. tCamens Q
G. Vessels Q
K. West
POLYOX TREATED AND UNTREATED S-G200 WET OPENING EVALUATIOH DATA
MultiMixer Pulped. 5 Min.
10 Min.
S-G200 Polyox Treated
1 Part/100 Viscosity
RPM cps
0.3 0.6
1.5 3.0 6.0 12.0
176,490 1*2,330
18,911* 10,889
5,993 3,321*
0.3 0.6
1.5 3.0 6.0 12.0
156,510
1*1*, 820
21,21*5 11,056
6,1*71* 3,371*
S-G200
Untreated
Viscosity
RPM
CPS
0.3 0.6
1.5 3.0 6.0 12.0
11*9,850
1*5,61*5 20,61*6 10,390
5,312
2,599
0.3 0.6
1.5 3.0 6.0 12.0
169,830
1*2,828
19,01*7 9,657 1*,797 2,64l
S-G200 Polyox Treated
10 Parts/100
128,205 1*5,650 16,850 10,023 1+.997 2,716
139,860 37,516 15,052 10,057 5,691* 2,999
5 Min. 10 Min.
PV YP AV
Ik 18 23.0 Ik 18 23.0
PV YP AV
12 16 20.0
12 17 20.5
PV YP AV
13 17 21.5
16 16 24.0
PV - Plastic Viscosity (cps)3 YP - Yield Point (lb./100ft. ) AV - Apparent Viscosity (cps)