Document g2q5ky95raDdn95qY9YmrMYaq

ST0 0 G7 8 4 3 BACKGROUND A. Types of Asbestos TLV,* Name fiber/cc Chrysotile 2 Amosite CrocUdolite Anthophyllite Tremolite 0-5 0*2 2 2 3Mg0-25:02'H20 (FeMg)SiO3 NaFe(Si03)2_FeSiO3-H2O (MgFe)7Si8022(0H)2 CA2MG5S18022^ OH >2 Most widely used form, KINKY FIBERS Known as "AFRICA* BLUE" B- Production of World's Supply Canada - 40% U-S-S-R- - 30% South Africa - 10% United States - 1-2% C- Uses - Asbestos is graded by length- Longest fibers go into TEXTILES, PACKINGS, BRAKE LININGS, AND ELECTRICAL INSULTIOttShortest fibers go into insulation cement, roof coatings, PLASTICS, AND CALKING COMPOUNDS- THE END USE OF ASBESTOS CAN HAVE A SIGNIFICANT INFLUENCE ON EXPOSURE HAZARD AND WHAT YOU SEE IN THE MICROSCOPE- D- Fiber Diameters - All fibers seen under simple magnification SYSTEMS ARE ACTUALLY BUNDLES OF FIBERS- To SEE A BASIC FIBER WOULD REQUIRE MAGNIFICATION OF ABOUT 50,000 POWER, OR THE EQUIVALENT OF AN ELECTRON MICROSCOPE- OUR COUNTING METHOD USES A MAGNIFICATION OF 400"450 POWER- *PROPOSED STANDARD OF 0-5 F/CC TWA AND 2 F/CC STEL PENDING ON CURRENT LEGAL APPEAL- 377374 BACKGROUND CONTINUED E- Changes in Standard 1. The odd TWA standard of 2 FIBERS/CC OF AIR IS CURRENTLY IN EFFECT AND WILL REMAIN IN EFFECT UNTIL LEGAL ACTION AGAINST THE NEW PROPOSED STANDARD is over- ; Current ceiling is 10 FIBERS/CC- 2- The proposed TWA standard is 0-5 fiber/cc with a ceiling of 5 fibers/cc- ! 3- 1972 1975 1976 TWA of 5 fibers/cc was standard OSHA proposed TWA of 0-5 fiber/cc NIOSH recommended TWA of 0-1: fiber/cc with 0-5 fiber/cc ceiling OSHA ADOPTED TWA of 2 fibers/cc with 10 fibers/cc I CEILING il il0L9001S 377375 IDENTIFYING ASBESTOS All methods below rely on the deflection of light passing through ASBESTOS, ALSO KNOWN AS REFRACTION OR REFRACTIVE INDEX- A MICROSCOPE IS USED IN EACH METHOD- A- Phase Contrast - Light from a bulb or other sources is con centrated (condensed) into a small beam which passes through the asbestos- The light beam then passes through doughnut SHAPED CONCENTRIC RINGS WHICH SEPARATE DEFLECTED AND UNDEFLECTED LIGHT WAVES, ALLOWING THE ASBESTOS TO BECOME VISIBLE- THIS IS THE CURRENT, DESIGNATED METHOD FOR COUNTING ASBESTOS FIBERS IN A SAMPLE- B- Polarized Light - Light is passed through a polaring filter WHICH ORIENTS THE LIGHT WAVES INTO A SINGLE PLANE- THIS LIGHT PASSES THROUGH THE SAMPLE BEFORE PASSING THROUGH A SECOND POLARIZING FILTER- THE ORIENTATION OF THE SECOND FILTER IS APPROXIMATELY 90 TO THAT OF THE FIRST AND ESSENTIALLY BLOCKS OUT ALL THE LIGHT WAVES WHICH WERE NOT DEFLECTED BY THE ASBESTOS FIBERS- T00670'i5 CO C- Dispersion Staining - The asbestos sample is stained and IDENTIFIED BY CHARACTERISTIC COLORS- THE METHOD IS COMPLICATED AND TIME CONSUMING, BUT MAKES POSITIVE IDENTIFICATION AND CLASSIFICATION OF FIBERS POSSIBLE- 377376 ST0067846 SAMPLING A- Equipment 1- Vacuum pump capable of drawing 1-7 Lpm of air against a RESISTANCE OF 6 INCHES OF WATER- DESIRED LENGTH, THI Cl WALLED RUBBER TUBING ATTACHED TO PUMP- 2- Filter membrane 37 mm, 0-8 micron porosity, plain white CELLULOSE ESTER MATERIAL- 3- Open face filter holder- Millipore 37 mm field cassettes ARE HANDY AND CAN BE REUSED IF WASHED IN WARM SOAPY WATERBand cassettes with tape or shrinkable bands to prevent air leakage- Use Leur slip adapters to attach hose to cassette- A- Bubble flow meter or a rotameter which has been calibrated WITHIN PAST YEAR- A RUBBER STOPPER CAN BE ADAPTED TO 3E CONNECTED TO A FLOW METER AND HELD IN PLACE AGAINST THE FILTER HOLDER WHILE MEASURING AIR FLOW- B- Procedure Try to obtain an 8-hour TWA as well as excursion concentrations WHENEVER POSSIBLE- A TWA SAMPLE SHOULD MONITOR AT LEAST 75% OF AN EMPLOYEE'S WORKDAY- Use A SAMPLE FLOWRATE OF 1 TO 2-5 LPM AND CHECK THE FLOWRATE AT LEAST AT THE BEGINNING AND END OF THE SAMPLE PERIOD- IF THE FLOWRATE HAS CHANGED USE THE AVERAGE FLOWRATE- Minimum desired sampling times can be estimated from Figure IIAn optimum sample WOULD have about one fiber per counting FIELD on the filter paper- 377377 377378 ST0067848 SAMPLE MOUNTING A- Items Needed Glass slides, 1x3 inch or 25 x 75 mm dimensions Scalpel or razor knife or razor blade or micro-scissors Tweezers Glass cover slips, ff 1-5 which are 25 mm Mounting solution - kept in refrigerator Lint free lens tissue Marking pen with fine point and permanent ink Filter sample Glass chips from broken glass slides "Bulldog" paper clamps Paper toweling B- Mounting 1- Cleanliness is next to important- Work on top of paper toweling, wipe glass slide and cover slip with lens tissue- 2- Work on one slide at a time until you are proficient- The first step is to label the slide with at least your name, SAMPLE NUMBER, AND DATE S' Remove the sample filter from its holder and cut out a wedge USING A RAZOR OR SCISSORS- Place 1 drop of mounting solution on the center of the slide in the form of an elongated bead- Place the filter wedge on top of the solution- 5- Outline the perimeter of the filter wedge on the underside of THE GLASS SLIDE- Be SURE NOT TO INCLUDE WITHIN THIS PERIMETER THE BASE OF THE WEDGE WHICH WAS HIDDEN UNDER THE FILTER HOLDER RETAINING RING DURING SAMPLING- 377379 ST0067849 SAMPLE MOUNTING CONTINUED 6- Place cover slip on top of filter wedge and place a glass chip ON TOP OF THE COVER SLIP- APPLY PRESSURE TO THE GLASS CHIP WITH A "BULLDOG" CLAMP ON EITHER SIDE OF THE SLIDE- Th IS IS THE PoETTCKER PROCEDURE- 7- Allow approximately 3 hours for the1 filter paper to become TRANSPARENT AND FOR THE MOUNTING SOLUTION TO HARDEN- PLACE THE MOUNTING SOLUTION BACK IN THE RFFRIGERATOR- 377380 ST0067050 ASBESTOS FIBER COUNTING PROCEDURE A- Method Specified by OSHA - Phase contrast illumination, 4 milli meter objective, 400-45QX magnification, binocular head, 10X Huygenian eyepieces recommended, counting field area of 0-003 mm2 or greater, Porton reticle recommended, etc- B- Set-up, Adjustment and Focus of Microscope 1- Set-up Position asbestos slide on "stage" (platform which holds slide)- Be sure 40X annular diaphragm and 40X objective are in proper position under and over slide respectivelyTurn on microscope illumination- Use coarse focus to raise the stage until it is^Va inch below the objectiveLook into the eyepieces and use fine focus to bring the sample into focus- 2- Adjustments Adjust distance between eyepieces to fit your eyes- Do this by pulling eyepieces apart and sliding together AGAiN UNTIL THE 2 ORBS OF LIGHT MERGE- THIS IS CALLED MARRIAGE OF THE ORBS- Isn't IT ROMANTIC! SHARPEN THE IMAGE OF THE PORTON RETICLE, WHICH IS LOCATED IN ONE OF THE EYEPIECES- SWITCH THE RETICLE TO THE OTHER EYEPIECE IF YOU DESIRE- ADJUST FOR DIFFERENCES IN SIGHT BETWEEN YOUR EYES BY FOCUSING THE EYEPIECES INDEPENDENTLY- FlRST CLOSE ONE EYE AND USE THE FINE FOCUS TO SHARPEN THE IMAGE' Then close the other eye and sharpen the image using the FOCUS RING AT THE BASE OF THE RESPECTIVE EYEPIECE- 377381 ST006785 I COUNTING CONTINUED 3- Focus Field Iris While looking into the eyepieces close the field iris APETURE ON THE BASE OF THE MICROSCOPE- USE THE CONDENSOR FOCUS KNOB TO BRING THE EDGES OF THE MANY"SIDED OPENING INTO AS SHARP FOCUS AS POSSIBLE- NOTICE THE INTERESTING COLOR CHANGES- ENJOY THEM, THIS IS THE HIGHLIGHT OF ASBESTOS COUNTING- OCCASIONALLY, THE MANY"SIDED OPENING WILL NEED CENTERING- Do THIS WITH THE TWO LONG"STEMMED KNOBS UNDER THE STAGE- OPEN THE IRIS JUST ENOUGH TO COMPLETELY LIGHT THE FIELD OF VIEW- C- Counting Count the number of fibers inside (see also half-fibers) at ,, Tf i^rvk "vi i.-i ,* fUt zo /Vf/cC tte Ltli'to. LEAST 20 DIFFERENT FIELDS-* A "FIELD" IS THE AREA INSIDE THE LEFT HALF OF THE PoRTON RETICLE- Keep counting fields until you have a total of 100 fibers or 100 FIELDS*/wHI*CHE^ER COMES FIRST- If &'-'^4^-7-^-*c; A FIBER IS TECHNICALLY ANY OBJECT WITH A 3:1 LENGTH"TO"WIDTH RATIO- IN REALITY FIBERS ARE FAIRLY EASY TO DIFFERENTIATE FROM BLOBS- Do NOT COUNT BLOBS, BUT DO COUNT RECTANGULAR OBJECTS WITH A 3:1 RATIO- 5Fiber length must be micrometers or longer- circle #6 IS APPROXIMATELY 5 MICROMETERS. The diameter of Do NOT COUNT FIBERS WHICH CROSS ANY TWO OF THE FOUR OUTSIDE boundari-es of the field- 377382 ST 0067852 COUNTING CONTINUED Half fibers - Count as a half-fiber any fiber which crosses ONE OUTSIDE BOUNDARY OF THE COUNTING FIELD- As AN ALTERNATIVE, PICK ANY TWO ADJACENT SIDES BEFORE STARTING AND COUNT AS WHOLE FIBERS ONLY FIBERS WHICH CROSS EITHER OF THESE TWO SIDESIgnore fibers which cross the other 2 sidesAvoid fields containing big clumps of debri which might hide asbestos fibersRecord fibers counted in each field on the attached sample record sheetChoose a new counting field as your record the fiber count from the last field- Do this by using your free hand to slightly twitch the microscope's lateral adjustment knobs- This technique randomly selects new fields- 377383 Fic 1 2 3 A 5 6 7 8 9 10 11 12 13 . 14 15 16 .17 18 19 20 ~ib3: Fie] 'ibe:i Km2' 221 O "TVl- (No. With >3:1 Ratio And At Least 5s In Lenath) T r~ '8E.AZ\s ''Los)Cq. 00348) Sample Nos- . 1 - 1 i -------- -- i , i I1 ri i f/ {i i\ it * i i ii I i t I * l 4 JI j i * j i 1 ! 1i1 ii 5j f1 ! ! i T Hours: Done By: Date : Checked E i 1 i1 i. 1t f i i 377384 1. ! . LA H o o ~ CO 04 ! 1 lV. ftfl ST0067054 DETERMINING MONITORING RESULTS A- Accuracy and Sources of Variation in Monitoring Procedure 1- Random Sources of Variation Intrafilter - Differences in fiber count from one area of THE SAMPLE WEDGE TO ANOTHER- Interfilter - Variation due to random fluctuations in PUMP FLOWRATE- Environmental - Variation due to random concentration CHANGES IN TIME AND SPACE- 2- Systematic Sources of Variation Intrafilter - Problem of air flow characteristics if use FILTER CASSETTES, AMERICAN INDUSTRIAL HYGIENE ASSOCIATION Journal (44), July, 1983, pg- 542-546- Intercounter - Differences primarily due to improper training, experience level, attitude, eyesight, and no quality control program- British study indicated untrained personnel obtained COUNTS 50-70% LOWER THAN TRAINED PERSONNEL- Interlaboratory - Variations due to differences in microscope QUALITY AND SPECIFICATIONS AND IMPROPER MICROSCOPE ADJUSTMENT- A NIOSH STUDY RANDOMLY TESTED 5 MICROSCOPES AND FOUND ONE CONSISTENTLY YIELDED COUNTS AN AVERAGE OF 45% HIGHER THAN THE OTHER SCOPES- Environmental - Systematic changes in concentration in time and space- 377385 ST0067855 RESULTS CONTINUED B. Field Calculations 1- Calculation of Total Number of Fibers on a Filter Fibers/(mm2 of filter) =Total ,fibers...................c.ounted (Total fields counted) (mm2/field) Where mm2/field = 0*00348 for the Olympus microscope in 1803 Building 2- Concentration of Airborne Asbestos Total Fibers on Filter = (Fibers/mm2)(855 mm2, for 37 m diafilter) Fibers = (Total fibers on filter) cc (Air flowrate, lpm)(duration, minutesHIOOO cc/liter) > > S'- C- Compliance Calculations 1- Compliance officer's test for non-compliance NC = (Sampled Air Concentration) - (1-645)(CV)(Standard) Where: (a) CV determined using Figure 3 (b) Standard temporarily 2 fibers/cc If NC exceeds the legal standard, then 95% of similar air CONCENTRATIONS WOULD EXCEED THE STANDARD AND A CITATION W'ULD BE ISSUED- | 2- Employer's Voluntary Test for Compliance IC = (Sampled Air Concentration) + (1-64)(CV)(Standard) If IC is less than the legal standard, then 95% of similarly measured air concentrations would be within the standard- 377386 377387 n * i fTOTAL FIBER COUNT >*1 Jo /> , Figure o " Tola! coefficient oi variation as a function of total fiber count (including pump error)