Document g2b59Mqqxr0L2Ry3aNpLE4O8G

1. askarels Meeting - Feb, 17 & 18, 1966 I* QUALITY IMPROVEMENT NEEDS: . A. Electrical Values Delivered to Customers 1) Resistivity 100oC. a) Capacitor Aroclor; 5, 000 X lO^ohm cm (Present min. is 500 X lO^ohm cm) b) Transformer askarels, 700 to 300 X lO^ohm cm. (Present min. is 100 X lO^ohm cm) 2) Power Factor lOO^C. , 60 eye. a) Capacitor Aroclor; 0. 15% to 0. 3% b) Transformer askarels; 1% to 3% (Present min. is 5% as we package but on reaching the customer it may be above 20%) 3) Power Factor 100 C. 1KC a) Capacitor Aroclor; 0. 02% to 0. 05% b) Transformer askarels; 0. 15% to 0.3% REMARKS: French, German, and Japanese askarels conform with the above as delivered to us. Evidentally, this holds also as usually delivered to their customers. While we can and at times do meet these levels on our askarels as freshly earth refined and placed in our storage--by the time our askarels reach the customers they are usually considerably off these guide lines. B. Biphenyl Content: Capacitor Aroclor: 0. 025% (250ppm) max. (Competitive material shows none to merely a trace of biphenyl. ) 0196775 TOWOLDMONOQ57311 2. Stability: Our present limits for capacitor Aroclor are: Aroclor 1242 Aroclor 1254 1) Hydrolysis 0. 5 ppm 1. 0 ppm 2) Westinghouse Test 1. 0 ppm 3) Monsanto (Thermal) 0. 4 ppm 0. 5 ppm 4) Thermal-chemical 0. 75 ppm Anniston material runs from occasionally the indicated maximum to usually 40 to 70% of the maximum values, depending on the individual test. More recently WGK has demonstrated their known ability to con form with the maximum limits. Given the right conditions, potentially WGK could do as well as Anniston. However, the stability analysis of competitive material indicates that the quality of our normally best Aroclor made at Anniston is not as good as comparable material from Japan, England, Germany, and France, as compared in this same order in the following table: \ 0196776 TOWOLDMONOQ57312 3. Test: Hydrolysis STABILITY COMPARISON of Foreign Made Chlorinated Biphenyl Aroclor 1242 Aroclor 1254 Kanechlor 300; 0. lppm Kanechlor 500; 0. lppm Pyroclor 1242; 0. 08 ppm Pyroclor 1254; 0. lppm Clophen A-30; 0. 04ppm Clophen A-50; 0. 17ppm Pyralene 1499; 0.04ppm --------------------------------------- Westinghouse Pyroclor 1242; 0. 30ppm Clophen A-30; 0. 20ppm Pyralene 1499; 0. 20ppm Monsanto (Thermal) Kanechlor 300; 0.2ppm Pyroclor 1242; 0. 09ppm Clophen A-30; 0. 09ppm Pyralene 1499; 0. 09ppm Kanechlor 500; 0. 2ppm Pyroclor 1254; 0.24ppm Clophen A-50; 0. 34ppm Thermalchemical Kanechlor 300; 0.42ppm Pyroclor 1242; 0. 19ppm Clophen A-30; 0. 35ppm ------------------------- -----------------. Pyroclor 1254; 0. 65ppm ------- -------------------------- -------- Pyralene 1499; 0. 17ppm ------- ----------------------------------- The above stability values appear 3 to 5 times better than our stability specification limits and in many respects 2 to 3 times as good as our best Aroclor made at Anniston. Accordingly, our stability goals needed to be competitive in stability quality appear clear and orderly. 0196777 TOWOLDMONOQ57313 4. II. EARTH TREATING EFFICIENCY: This is directed at moisture removal and improvement of Power Factor and Resistivity. It is not known whether we use the best available earth refining pro cess. Variables are type earth, minus 200 mesh versus 60/90 vs 30/60; drying to below 1% moisture; conditioning temperature; amount of earth; temperature and time of treating; method of treating, i. e. , batch versus percolator; earth removal; storage of conditioned earth. III. NEED TO CLEAN UP TCB and TTCB ELECTRICALLY There are no electrical quality specifications applicable to Hooker supplying TCB and TTCB for transformer askarels. At prevailing prices Hooker is not receptive to such restrictions. The electrical properties of our incoming chlorobenzenes are quite bad and we do not check them. It would seem prudent for us to earth refine these materials, check the results, and not use them if they do not respond satisfactorily. IV. PACKAGING: A. Merits of Hot Packaging? It helps eliminate moisture problem in our factory and would seem to create the moisture problem at the user end, if the material cools in storage and transit. 0196728 TOWOLDMONOQ57314 B. Contamination . 1) From loading lines and pumps 2) From the packages 3) From taped sample bottles C. Drums 1) Are our drums adequate for international shipment? 2) One coat phenolic vs two coats phenolic formerly used vs galvanized formerly used, vs galvanized 16 gauge and rolling rings used by Bayer. 3) Bung gasket material? 5. V. TEST METHODS A. Electrical Tests 1) Power factors and resistivity methods, WGK versus Anniston versus customers 2) Need for capacitance standard to check bridges. 3) Anniston was reading low power factor and also resistivity incorrectly. 4) Both Anniston and WGK probably would read high power factors incorrectly. 5) Need PF and Resistivity procedures properly written for customer use, especially international. This is directed at instructions that might give chance for customer correlation with our methods. 0196774 jf/1/10/66 Paul G. Benignus TOWOLDMONOQ57315