Document emGJ3BZvJ9pn12rnGG54N20N4
Deterioration of Alkyd Resin Films
EMERSON B. FITZGERALD
Marshall Laboratory, E. /. du Pont de Nemours & Co., Inc., 350% Grays Ferry Ave., Philadelphia 46, Pa.
THE organic chemistry which is involved in the photooxida- cases where a borosilicate glass filter was used the energy was tive deterioration of an alkyd resin is known to be vastly about one third of this value. Air was circulated about the tubes complex. While much attention is being given to fundamentalby a fan, and thermometers that were placed inside with the
investigations of oil oxidation by laboratories concerned with the specimens stayed at 30 C.
study of edible fats, there are numerous points of interest relating
Each run began with the light on but with no specimens in
to alkyd resins which may be attacked in a less rigorous manner. place; gas was passed through the system at 5 cc. per minute until
One such problem is concerned with determining some of the constant weight was obtained in all adsorption tubes. The se
simple kinetic relationships and over-all physical results of the lected specimens were then inserted; the light was turned off, and
action of light on an alkyd film. The purpose of the present gas flow was continued until constant weights were again at
work, which was carried out as part of a larger investigation, was tained. At tins point the light was turned on and weighings of
to determine the rate, the geometrical location or site of attack, all adsorption tubes were scheduled on a daily basis for usually 7
its approximate relationship to wave length, and its dependence days. At the end of the run the panels were removed and
upon oxygen concentration.
weighed, and in some cases scrapings were analyzed for carbon
Two very simple and straightforward experimental procedures and hydrogen.
were used throughout the work--measurements of volatile de
composition products and microinterferometry of the surface.
MEASUREMENT OF VOLATILES
Analysis of volatile decomposition products arising from decomposing linseed oil or alkyd resins is by no means new (?, 4, 6). In none of the previous work, however, was any attempt made to use films of precisely known area, weight, and thickness, so that no real estimate of the rate and locus of attack could be made. Further, all of the previous work had been directed toward the very early changes in liquids or wet films. The pres ent effort, on the contrary, is concerned wholly with hard, baked film, and the course of gas evolution is followed up to and beyond the point of easily visible chalking in the case of pigmented films and to corresponding extents obdeterioration in the case of clear films.
APPARATUS AND PROCEDURE
The resins to be studied were sprayed on weighed glass panels all 15 X 2 cm. The panels were baked 1 hour at 105 C., aged for from 1 to 3 weeks in the dark, and reweighed. Film thick nesses, in terms of milligrams per square centimeter, or the reciprocal, were calculated from these data; a wide range of thick nesses was prepared, and only perfect panels (smooth even films) were selected for use.
The exposure vessels were quartz tubes, 25 mm. in outside diameter. At one end sealed inlet tubes were connected to a purifying train that removed Carbon dioxide and water from the tank gas being fed into the tubes; at the exit end the tubes were equipped with standard-taper openings, capable of admitting the specimen panels. A gas absorption train consisting of a pair of Pregl tubes (Dehydrite and Ascarite-Dehydrite), a microcombus tion furnace, another pair of Pregl tubes, and a bubble counter was attached to the exit end of the exposure vessels.
A Hanovia Utility lamp--medium pressure quartz mercury vapor--was positioned symmetrically above the horizontal ex posure tubes that were always used in pairs. In order to ensure even illumination the lamp was frequently moved a few milli meters in random directions; in this way the effects of hot spots in the lamp and flaws in the quartz exposure tubes were mini mized and pigmented panels so exposed gradually acquired an even coat of chalk. The lamp-to-specimen distance was held constant at 10 cm. throughout the work; the total intensity actually received by the panel was estimated from thermopile measurements to be approximately 0.05 watt per sq. cm. In those
Figure 1. Gases Evolved from Baked Alkyd Film upon Exposure to Ultraviolet Light in Oxygen
The resin used in most experiments was a linseed-chinawood oil alkyd of 50% oil length and an acid number of 18. When used with no modification other than a common drier this is referred to as "clear alkyd." In some experiments this same alkyd was pigmented at 20% by weight with titania, and this is indicated where it occurs in the results.
Figure 1 shows the averaged results of three separate runs on the clear alkyd. The term "precombustion" used in the figure refers to gases collected in the adsorption tubes preceding the furnace and immediately following the exposure tubes. The "postcombustion" gases were, of course, collected in the final pair of adsorption tubes. The large ratio of carbon dioxide to water in the postcombustion gases indicates a high proportion of carbon monoxide in the gas entering the furnace.
The decrease in the rate of water evolution in the precombus tion gas, which results in an intersection of its curve with that of carbon dioxide, is a typical result, except that in most cases it occurred before 100 hours. Careful examination of the figure reveals that the rate of carbon dioxide evolution is also decreasing, though much more slowly. A few experiments conducted for a longer period of time revealed this decrease more clearly; the total effect is sufficient to denote a drop in the over-all rate of reaction.
2546
INDUSTRIAL AND ENGINEERING CHEMISTRY
Vol. 45, No. U
It 13 possible that some contribution to the rate decrease, par ticularly that observed in the data for precombustion gases at about 20 hours, was due to disappearance of traces of solvent which may have been in the film at the start of the experiment. If this were* the case, it must also be concluded that the solvent vapOr (all hydrocarbon) was oxidized to carbon dioxide and water while still in the irradiated region. Otherwise it is unlikely that the rate change would have been observed in the precombustion gases; it would, instead, have occurred in the postcombustion data, which are seen to be nearly straight in this region. In any case; traces of solvent, if they exist, may be regarded as no dif ferent from any other low molecular weight or easily oxidizable constituent of the film.
Figure 2. Gases Evolved from Baked Alkyd Film in 100 Hours of Exposure to Ultraviolet Light and Oxygen
OO Clear alkyd # Alkyd and rutile 99 Alkyd and anatase
Unfortunately, there is no way of inferring from these data the true initial products of the photolysis. The slow sweep of gas through the train undoubtedly allows time for the photooxidation of volatile products such as aldehydes and ketones if any occur. While a knowledge of the initial reaction products would be of value in elucidating the chemistry of the process, the lack of this information is not a handicap for the purposes of this investiga tion.
Figure 2 shows the combined post- and precombustion gas evolution as a function of film thickness. Here the ordinate gives the weight of gas evolved from each square centimeter of film and the abscissa gives the initial weight of pure resin in each square centimeter of film. The equation of the experimental lines is:
s--q. c-m-. = As..q..--cm. + B
(1)
where w is the weight of gas and W is the resin weight. In the case of clears, W is, of course, identical with the film weight, but with pigmented specimens it is equal to 0.8 of that amount.
It is evident from the experimental points that in this test there is no distinguishable difference between clear and pigmented films nor between rutile and anatase pigmentation. Also, it is clear that since a film of zero thickness (TF ~ 0) can evolve no gas, the intercepts (B) cannot exist. In fact, the limit of permissible values must be given by the weight of gas which could be evolved upon complete combustion of the film. This theoretical limit is given by the dotted line in Figure 2 and was calculated from the fact that the resin used in these experiments would, upon com plete combustion, yield 254% carbon dioxide and 62% water.
Assuming then, that the line representing the total gas inter cepts the theoretical limit and follows it down to the origin, the abscissa of the intersection gives an estimate of the depth of film that has been quantitatively eroded from the surface in 100 hours. This amount is found by calculation to be approximately 2 microns.
The continuing upward slope of the data at greater film thick nesses is a measure of the extent to which the underlying layers of resin are contributing volatiles, possibly including traces of resid ual solvent, to the total amount collected. It seems likely that this relatively slower process in the depth of the film is due to radiation of longer wave length, which is not filtered by the top most layer. If this is true, then the decrease in reaction rate that is observed at longer periods of time may be interpreted in two ways:
1. As the surface erosion due to the short-wave ultraviolet pro ceeds into the film it eventually reaches underlying resin that has been subjected to long wave irradiation for a considerable period of time and as a result has been chemically converted into a more stable form.
2. The other possibility is that the reaction at the surface is not quite quantitative and, as the erosion proceeds, a layer of unreactive debris that acts as a shield is left on the surface.
It is likely that both of these effects occur and that the relative importance of each depends upon whether the film is clear or pig mented. In either case it is reasonable to assume that the rate of initial gas evolution would be decreased if the film were baked an extra-long time prior to starting the ultraviolet exposure. This was tried and found to be the case.
In addition to the experiments using the unfiltered Hanovia lamp with an oxygen atmosphere, a few runs were made using dither a borosilate glass filter that excluded short wave lengths, or an atmosphere of purified, dry nitrogen. Results at 100 hours for two typical experiments are:
Pigment
Rutile Anatase
Film Thickness, AfcmosMg./Sq. Cm. phere
13.8 6.1
N* Os
Filter
None Borosilicate
glass
Total Gas EvoLved, Mg./Sq. Cm.
CO HsO
0.13 0.14
0.22 0.11
Comparison of these data with those of standard runs shown in Figure 2 reveals that while the reaction is greatly retarded by either a filter of nitrogen, it is by no means negligible in either
The rate of chalk development during all of the foregoing experiments in which pigmented films were used was qualitatively observed to be dependent upon the exposure conditions in a most significant way. With the use of unfiltered light and dther nitro gen or oxygen atmosphere the. first easily perceptible chalk ap peared after the evolution of approximately 0.2 mg. of combined gases per sq. cm., while with filtered light no chalk appeared even at higher levels of gas evolution. This seems to confirm the idea that unfiltered ultraviolet gives a highly erosive surface reaction combined with a bulk reaction, while light from which the
Ta b l e I. Hy d r o g e n t o Ca r b o n At o mic Ra t io s Av e r a g e d f r o m Se v e r a l So u r c e s
Number
Litera
ture Cited
Material Used
Experi
In
ments original
Averaged material
Linseed oil
Linseed oil Trilinolenin Linseed oil
+ ZnO
Linseed oil
+ TiO, Alkyd
9 8 4 8
12
3*
1.76 1.76 1.62 1.76
1.76
1.20
a Data taken from Figure 1 at 140 hours. k Analysis on only one specimen.
H:C Ratio
In off gases
3.89 0.35 3.22 0.34 2.01 0.23 4.33 0.15
In residue
Not given 1.74* Not given Not given
4.60 0.30
2.50 0.40
November 1953
INDUSTRIAL AND ENGINEERING CHEMISTRY
2547
short-wave radiation is removed produces chiefly the bulk reaction that leaves the surface relatively intact.
If it is correct, as implied above, that the radiation of longer wave length produces chiefly a bulk reaction, then it follows that thermal oxidation of alkyd Aims should be solely a bulk reaction. Eigure 3 shows the results of a series of thermal oxidationmeasure ments in which panels prepared in the same manner as before were
Figure 3. Weight Loss from Clear Alkyd Films in Air Oxidation
O Glass substrate Aluminum substrate
as postulated above, the gases obtained under such conditions should have more nearly the composition of the whole resin.
Dehydration has also been observed in oxidation studies on pure compounds. For example, Treibs (S) found that methyl oleate evolves 1 molecule of water on exposure to air in thin films and methyl linoleate evolves between I and 2 moles per mole of ester. One possible mechanism may be that shown in Reaction 1.
------ d)------ djsrsd)------ s= ------ O------d)=Cr--
-f h 20
ooh
o
(1)
The quantity of carbon dioxide evolved in all experiments except those using the thickest films was far too large to be attrib uted to simple decarboxylation of free --COOH or to any other angle functional group in the molecule. It must be concluded, therefore, that the carbon dioxide (and carbon monoxide) results from chain scission reactions that may originate from hydroper oxide decomposition in the oil and probably also from reactions of complex nature occurring in other parts of the alkyd molecule.
In a study somewhat similar to the present one, except that it was conducted on Buna rubber in vacuo, Postovskaya and Kuz'minskil (5) found a quantum yield of 2 X 10"* for the over all photoreaction evolving volatile products. They interpret this low value as proof that the deterioration is not a ch&in reac tion. Bateman (/} likewise found a very low quantum yield (4.0 X 10~4) for the gas reaction in the photolysis of rubber but did not interpret his result. While the present work was not designed to permit an accurate calculation of the quantum effi ciency, a rough estimate may be made with the aid of a few as sumptions. Thus, if it is assumed that wave lengths from the lower limit of the lamp (about 2500 A.) to only 3200 A. are effec-
heated in an air oven. This time, however, the volatiles were not caught; instead, the remaining film weight was recorded as a function of time, temperature, and initial thickness. While this method of conducting the experiment is~ not strictly comparable with that used previously, it clearly indicates the bulk nature of the thermal reaction and lends support to the idea that light in thejlonger wave lengths produces only a bulk reaction.
DISCUSSION
Some insight into the chemical nature and mechanism of the
X processes by which volatile products are evolved may be gained
by examining the hydrogen to carbon ratios of the gases as com-
J pared with that of the original film. Fortunately, several of the
references cited previously (2~4, 6) contain data from which these
Bame ratios may be computed. The comparison is given in
Table I.
Apparently there is-general agreement that the volatile decom position products are hydrogen-rich compared to the parent ma gisterial and the hydrogen-carbon ratios of residues are practically
ll'nnchanged. However, for small-to-moderate amounts of de c|olsmenpsoitisvietioton tchheanhgyedsroignenth-cearcboomnproastiitoioonf othfethreesiodfuf-egaiss vaenrdy.inno-
.imdue importance should be attached to the two values listed in
fthe. table.
The hydrogen-carbon ratios of the off-gas are certainly signifi
cant and prove clearly that dehydration is an important step both
in, the mechanism of drying
#) &nd hi the deterioration of
, completely dried films as shown here. Corresponding ratios
|ound in the present work using, the borosilicate glass-filtered
fight or nitrogen atmosphere were, in general, higher and averaged
tween 6.0 and 7.0. This is as it should be, for if the surface
Action initiatedrby^short-wave ultraviolet is nearly quantitative*,
Figure 4. Interference Fringe Shift between Xrradiatedandllhi^admt^
I;
j
t ii i
i\ !i: \
:if
ji
i i!
! l
2548
INDUSTRIAL AND ENGINEERING CHEMISTRY
Vol. 45, No. U
tive and that all the radiation in this region may be averaged at 2800 A., then the most serious shortcomings are over. The energy emitted by the lamp used in the present work, within the specified range, was estimated from thermopile measurements using cutoff filters, to be about 0.01 watt per sq; cm. at the actual distance used in the experiments. If we neglect surface scatter ing and assume complete absorption, this amounts to about 1.4 X 10i6 quanta per sq. cm. per second. Using the fact that the film thickness in the experiments averaged in Figure 1 was 5 mg. per sq. cm, one may calculate from the data shown there the rate per area evolution of gas molecules of each type. Taking the values at 100 hours and adding the rates for all types of molecules, the result is 1.4 X 1012 molecules per sq. cm per second. Thus, the estimated quantum efficiency is 1 X 10 "*4.
While this result agrees in general order of magnitude with the previously mentioned values for Buna rubber and rubber, it would appear that the situation is too complex to attempt any subtle inferences. It may be safely concluded, however, that in retrospect hardly any other value of quantum efficiency could have been expected from a material which has been used success fully as an exterior protective coating for so many years.
INTERFEROMETRY
Additional information regarding the surface attack of light and oxygen on a hard smooth film may be obtained by well known techniques of mterferometry. Optical details may be found in Tolansky (7). Panels were prepared by doctor-blading the resin, clear or pigmented, on plate glass and giving a standard bake. Double-edged razor blades lying on the film were used to give sharp lines of demarcation during irradiation. After the desired exposures had been given, the blades were removed and the entire panel was silvered by vacuum evaporation. Interferographs were made at the boundaries, previously formed by the razor blades, between exposed and unexposed surface. Ob viously, if erosion had occurred, a step would be formed whose depth could be determined by measuring the shift in the Fizeau fringes. . A series of exposures ranging from 8 to 48 hours was carried out according to this plan, using the unfiltered lamp and air atmosphere. Figure 4 is a typical example of the steps that were found. The height of the steps was estimated from the fact that one full shift of a band corresponds to one half the wave length of light used in making the photograph or about 0.25 micron for the mercury green line that was used here. Results of these measurements showed that the depth of each step was approximately proportional to the time of exposures and that the rate of surface erosion was about 1.5 microns per 100 hours. While this value is somewhat lower than that obtained by the gas
analysis method, the agreement seems satisfactory in view of the approximations that had to be made in both methods.
SUMMARY
The decomposition of an alkyd film by light below 3000 A. in a stream of dry oxygen appears to be a nearly quantitative combustion which ultimately yields carbon dioxide, carbon monoxide, water, and small amounts of other volatiles. This reaction occurs in an extremely thin surface layer which dis appears as the reaction proceeds and, in the case of pigmented films, produces chalking. The rate of penetration of this sur face erosion can be estimated from gas analysis data or micro interferometry.
In addition to the surface reaction there is a bulk reaction that extends throughout the depth of the film and that must be essentially a dehydration or dehydrogenation, since the atomic ratio of hydrogen to carbon in the mixed gases is much higher than it is in the pure resin.
The rate of gas evolution decreases slowly with time, indicat ing that a new and more stable structure is being formed. The rate with films containing 20% rutile or anatase pigment is about 20% lower than it is with clears, indicating that, to this test, the pigment is an inert space filler.
A similar (Quantitative surface reaction occurs when the radiation with light below 3000 A. is carried out in a stream of pure, dry nitrogen. The rate of gas evolution in this case is much lower, however, and the oxygen in the carbon dioxidewater mixture comes from oxygenated groups in the resin. With pigmented films, chalking appears at about the same point in the reaction as it does in an oxygen atmosphere as measured by the weight of cqmbined gases evolved, but the atomic ratio of hydrogen to carbon is much greater, and yellowing increases.
When all radiation of wave lengths shorter than 3000 A. is removed from the light, the erosive surface .reaction is greatly surpressed while the bulk reaction continues to produce carbon dioxide and water at a slow rate but with a high hydrogen-carbon ratio.
LITERATURE CITED
(1) Bateman, L.t J. Polymer Sci.$ 2, 1-9 (1947). (2) D'Ans, J., and Merzbacher, S., Chem, Umschau, 34, 283-91,
296-304 (1927). (3) Hedvall, J. A., and Helander, H., Arkiv Kemi, Mineral. Geol.,
17 A, No. 22, 1-16 (1943). (4) Long, J. S., Rheinbeck, A. E,, and Ball, G. L., Jr., In d . En g .
Ch e m., 25, 1086 (1933). (5) Postovskaya, A. F., and Kuz'minskil, A. S., Zhur. Fiz. Khim., 25,
863S (1951). (6) Slansky, P., KoUoid-Beih., 35, 49-88 (1932). (7) Tolansky, S., "Multiple Beam Interferometry of Surfaces and
Films," London, Oxford University Press, 1948. (8) Treibs, W., Per., 75, 203, 632, 953 (1942); 76, 670 (1942).
Re c e iv e d for review May 7, 1953.
Ac c e p t e d August 1, 1953.
Presented in part at Gordon Research Conference, New Hampton, N. H.,
June 1952.
,
^