Document e6BRLxL9Ma9ngddrQOkGEGrg

Chemicals - Plastics .> . . '^r*. t. . ^MONSANT6 i*LASTICIzifK in Synthetic $.eiin aidheiivei Monsanto Technical Bulletin No. 0-99 April, 1953 Monsanto Chemical Company, Organic Chemicals Division, St. Louis 1, Mo- iNTRODUCTION The superior properties of plasticized synthetic resin adhesives are causing these pre parations to rapidly displace or supplement conventional animal and vegetable base ^ -adhesives. ^The synthetic resin adhesives referred to are primarily adhesives based on : --polyvinyl acetate and its co-polymers with polyvinyl chloride or polyvinyl alcohol, but also included are adhesives with such bases as nitrocellulose,^in, casein, aery - lates, polystyrene, cellulose and other polymers. v Synthetic resin adhesives find a wide and increasing usage in such diverse industries as the following: . - - ,trrfy-- ' Shoe industry _ Book binding industry Paper Bag sand folding box carton manufacturing Sanitary food container producers Ltminatorvatad coDverters of packaging products ; - Tofacco industry ^packaging) ' ,v- . ^Automotiveindustry _ Foodindustry {for labels and carton teajjpg), ate. . #3 Factors contributing io the sapid increase in the quantityflae of synthetic1Tain ad- Ww"`taew^ .. 1) -Synthetics are better adapted to high speed machinery operation and make . up their increased cost over other adhesive types by the resultant increases ' fa production aates. ^>%g :; v a -- ^ 4 - 2) Bynthetk adhesives are cleaner and easier to use from a production and " wnaintrnsnrr islandpniiK ; v ~ .. - ii. . .t-c '-..uU.;* ak< . - ik . ? i J) MSynthetk^Adhenves !fcave auperior water, anold sd 4uagusWMistance and t - of fleidl^tyaanlbeofetained." . .- -v- ** ^ 'aABierivr^^aMus olmate she^useof vokrik toxic^ .................. 3 mw&fi '->5** *-<: v>0 *< 2 *3 *o 5 o STLCOPCB4092341 WSSSgga`S '.'- v<y. TYPES 0F&RES1N ^ADHESIVE FORMULATIONS "The Tfiajor typ& fir^felidal^^t&Bc'^ln^^Uwsive formulations are A, Emulsion; B, Hot-melt; C, De- ^Tayed-taxiViD, `Solvent;' F, Adhesive Primers or Coatings. These will be discussed - in order. TJnits forall formulations are weight percent or parts by weight. Sources of ingredients are listed at the back of this bulletin. v, ' v . -- . ...: ..-.. a. Emulsion Adhesives " Resin emulsion adhesives are emulsions of /plasticized resins dispersed in a water base. They are often ex tended with materials like starch paste and thus require the incorporation of a preservative. The resin most commonly used in emulsion adhesives is polyvinyl acetate. The following is a typical polyvinyl acetate emul sion adhesive formula: . .. ...... A.-l. Polyvinyl acetate emulsion (55% solids) Pi[ `l=astic izer'. ' - . Clay Filler - Corded/starch or dextrine Preservative '> ' "... - Stabilizer Wetting Agent ? !' 3 ^ .Secondary water ... . Defoamer Odorant -(masking agent) W 100 10 -so . 0 -30 0 - 1,000 ' 1-2 1 -2 0 -0.2 75 -100 1-2 0 -1 The plasticizers most commonly used in polyvinyl acetate emulsion adhesives are dibutyl phthalate and orthonitrobiphenyl (ONB). ' Dibutyl phthalate imparts good flexibility and softening action with relatively low volatility! ONB is hot quite sis efficient as dibutyl phthalate as a plasticizer, but is widely used because of its economy as cither an ``extende^jiiasticizer or as the sole primary plasticizer. Dimethyl phthalate is used in some cases because of its low cost and because it is a better solvent for bond ing to cellulose acetate film.or sheeting -where .ihis material is used, in making windows in or laminations to jpaper. Tricresyl phosphate and Santicizer*140 are used where flame resistance, oil resistance tand low vola tility are desired. Santicizer'liO is'tnore efficient than TCP and has better light stability and less odor! <Santicizer M-l 7 -is an excellent plasticiser .for /bonding acetate overlays to paper, /because of its /superior light jility.sSantidzi^S fmparts jgood/llqsrsand wetting action and has' excellent grease resistance. fi8Mitjjcir , ,M60 is -consideredin foot applications than dibutyl phthalate because of its lower volatility,greater iilm toughness and Improved moistuirelie^anoef' "* ' ' " 1 ' A'* ' v - .<1 aticizer, aye been granted approval^ arsssvsi i-AUi r* nontoxic applications ;j(fbod " tbthunref-a.umomf ----fc films DSW 587008 STLCOPCB4092342 A. Emulsion Adhesives (continued) Monsanto industrial resins, Santolite* MHP and MS-80%, are the best resin additives for use with poly vinyl acetate for imparting quick tack. They are being used successfully for bonding cellophane to cello phane and aluminum foil to paper. These resins make a very tough but flexible adhesive and are normally compounded with some liquid plasticizer like dibutyl phthalate, or with an eutectic mixture (1:1) of dibutyl phthalate and triphenyl phosphate. The table on page 5 gives data evaluating various Monsanto plasticizers in combination with polyvinyl ace tate. Properties evaluated are compatibility, volatility, low temperature flexibility and grease resistance. It will be noted that the typical emulsion adhesive formulation A.-l requires a preservative. Monsanto sup plies an excellent line of industrial preservatives which includes Santobrite*, Santophen* 20, Milmer*I and these masking agents: methyl salicylate, Santomask*, saccharin, coumarin and vanillin. Literature on these products is available. At the back of this bulletin is a listing of the various trade marked products men tioned in succeeding formulas. Formulas A.-2 and A.-3 below are more examples of polyvinyl acetate (PVA) emulsion adhesives. A.-2. Quick Tack PVA Emulsion Adhesive Gelva Emulsion S-S6 (51% solids) Dibutyl Phthalate . Santicizer* 8 Water 100 11.8 11.8 9.4 ' Through the use of other additives, adhesives designed for specialized purposes may be formulated. As an example, the following formulation shows good properties as an adhesive for bonding moistureproof cello phane to aluminum foil or to paper; or for bonding aluminum foil to paper. A.-3. Polyvinyl Acetate Emulsion Adhesive Gelva Emulsion S 55** Dibutyl Phthalate Santolite* MS-80% Water 100 ~ - ' ... -.9 , 13.5 .. . "13.4 v: > if This formulation shows rapid development of adhesion and bond strength at elevated temperatures. . *''**? The following formula is an example of a low molecular weight stymse yokyicr STLCOPCB4092343 >V'- A. Emulsion Adhesives (continued) A.-4. Styrene Emulsion Adhesive HB-40* Diethyl Phthalate Triton X155** Lustrex* Styrene 601-40 Ammonia Caseinate,"15% 18.0 6.0 2.5 100.0 34.0 Formula A.-4. illustrates a basic, stable composition which possesses a high degree of wet tack. Such prop w erties as stability, wet tack, and film toughness are imparted to this composition by the caseinate present and are varied by changes in the caseinate ratio: The following formulation is suggested as a grease-resistant coating for paper products for wrapping such items as bakery goods. ` A.-5. Polyvinyl Acetate Grease-resistant Paper Coating Elvacet 81-900** Santicizer* B-16 Tri-Pure **(titanium dioxide) . Water Quilon** . '' 100 3.5 7.0 15-30 0-5 The above composition is applied with a Toll coater provided with a smoothing roll to develop a uniform con tinuous film. If used as a laminating adhesive, about 140F. heat is required for optimum film formation. .. 1 fl' Ifii ' i B. Hot-melt Adhesives Hot-melt adhesives may be made with either liquid or solid plasticizers, depending upon the properties desired in the end product. Santicizers* M-17 and 160 and dibutyl phthalate are favored because of their excellent heat stability and mild odor. Of the solid plasticizers, diphenyl phthalate and Santicizer 1-H are preferred because they have the least odor and are in the proper melting point Tange for most applications. Three formulations are given (all parts are by weight or in weight percent). ' `' B.-l. Hot-melt Coating Cellulose Acetate Santicizer* M-17 Inert fillers 50 88 35 B.-2. Hot-melt Bookbinding Adhesive Neville Hafdltesin** '' 61.4% Mix and heat ; Santicizer 160* 1` 15.0% at 250-Z75F. Paraffin wax . . . . .. . 6.4% until melted. " Blaise temperature to 300-325F. iand agitate-after adding: isrf.fs v i.- ' ATmylite AYAA (polyvinyl acetate) ,. < 12.9% ";EEtthhyvll cceelllluulloossee -> riyvi ; :Hr, * "4.3% cm* '^Bookbinding Mot Melt ^application <temp.:;165175?F.) 100 JO-79 * V`4! StrfT $04$ il`h ! STLCOPCB4092344 ; Delayed-tack Adhesives ' These preparations, after they are spread and dried on a surface, are normallytack-free at Ordinary^tempera l tures. They are activated by heat and possess the property of maintaining .tackiness over a fairly wide tem perature range from several hours to several days. This permits the necessary mechanical handling, while two surfaces are being united, before the adhesive becomes nontacky by cooling and setting., Thus, the action of delayed-tack adhesives differs from that of hot-melt adhesives where tackiness terminates on cooling alone. Solid plasticizers, such as diphenyl phthalate and Santicizers* 1-H and 9, make possible the "delayed-tack" feature of these unusual adhesives. Plasticizers are selected on the basis of their effect on the:base resin (i.e., the temperatures at which the adhesive quality is activated and de-activated), and for -their heat and Tight stability, odor, nontoxicity where required, etc. Much of this art is described in the patent literature (for example, U.S. patents numbered 2,462,029; 2,608,542; 2,608,543; 2,613,1S6 and 2,613,191) which should be investigated by those desiring to produce delayed-tack adhesives. Sample formulations below were taken from such patents, as indicated. , Example 9b Delayed-tack Adhesive (from U.S. -Patent No. 2,462,029) Santicizer* 1-H Vinsol Resin Thinned Amine Dispersant Acrysol M.R. 50 50 240 10 "The thinned amine dispersant is a mixture composed of 1 part stearic acid, 1 part "polypale resin", a polymerized rosin containing approximately 40% dipolymers of abietic acid (Hercules Powder Co.), 1 part of 2amino-2methyl-l propanol (Commercial Solvents Corp.) and 3 parts of water. This com position is designed solely as a dispersing assistant ..." % -I^From Column 10 of above patent. ' C ... : .. . ' Example 18 Delayed Tack Adhesive (from U.S. Patent No. 2,462,029) Diphenyl Phthalate Nevindine R-3 Thinned amine dispersant (see above) Hycar OR-25 _ ........ 52.5 30.0 198.0 43.5 - The above formulation is nontacky at ordinary temperatures and is heat activated at about 150F. The compound will then remain adhesive through temperatures as low as 50F. Once set, the ad hesive continues to hold at ordinary temperatures. C.-3. Polystyrene Emulsion Delayed-tack Adhesive (Example I of U.S. Pat. No. 2,613,156) ' "Ten (10) parts polystyrene (molecular weight 10,000 - 15,000) and 40 parts diphenyl phthalate are mixed and heated together at approximately 190F., forming a clear fluid. While still at this temperature, the fluid is poured into a solution of 6 parts of a .25% aqueous solution of Aerosol OT and 4.5 parts polyvinyl alcohol (of the grade sold underthetrade name of Elvanol 50-42) in 75.5 parts water; the solution being at a temperature of approximately 190F., constant agitation is maintained, resulting in a homogeneous emulsion. The emufeiohas then permitted to cool."%This formulation is improved by the addition, after cooling, of 8 parts of Geon polyblend 550X20.) ;r-- /- - This will form a smooth nongrainy film when spread evenly on paper, and-j^klby to a^completely tack-free ^surface. When heated to 170F., the film becomes very tacky and powerfullyiadhesive?^taining these prop-' Gerties formas hmg as 90 seconds while cooling.1 1 '' ' . * - !. ..... ___ ....... ^ safj DSW 587011 i STLCOPCB4092345