Document e5yM6wYQjdpbgOne13m7eRnM9
If Monsanto Chemical Company Organic Chemicals Divisioi North LIndberg h Blvd. ... St. Louis 66, Missaur
JkoCHEMICAL SPECIALTIES DAT..A......R....E...P...O...
The information in this report was compiled to assist you in your evaluation and development of special uses for Monsanto products. Kvory effort has been made to include pertinent material hearing on the subject. This information is intended
to guide your development work, but Monsanto cannot take part in the specific formulation or evaluation of any finished product . . . since knowledge of such should be reserved to yourself and is often your most valuable trade secret.
No. Date
CS-14 November, i960
AROCLOR* FIRE-RETARDING PLASTICIZERS AND MODIFIERS FOR EPOXY RESINS
Because of their outstanding chemical resistance and adhesive char acteristics, epoxy resins are widely used for the production of surface ooatlngs, adhesives, laminations and plastic parts.
To Impart flame resistance -- with attendant lowering of cost -Aroclor compounds oan be added to the resins in various proportions. The flame retardant resins so produced have many Important uses. In laminations and plastic parts, for example, it is often necessary or even mandatory that flame resistance be built into the finished product.
By selecting the proper Aroclor, formulators. can meet requirements for fire resistance while, at the same time, adjusting such other important properties as flexibility, hardness and viscosity.
Chemically, the Aroclor compounds are dl- and poly-phenyls chlorinated to a definite per-cent-by weight of inert, bound chlorine. Physically, they range in form and appearance from Aroclor 1221, mobile oily liquids, to Aroclor 5460, hard transparent resins. Chemically, the Aroclor compounds are impervious to moisture, acids and alkalis; they are extremely heat stable and will not support combustion. When added to resins, the Aroclor compounds function as low-cost plasticizers imparting fire-retardant properties to the resin formulation as well as other desirable end-product characteristics.
This report covers the application of Aroclor plasticizers in epoxy resin formulations.
0019169
* Aroclor is a trademark of Monsanto Chemical Company for its ohlorlnated aromatic hydrocarbons and their derivatives, including chlorinated diphenyl. Reg. U. S. Pat. Ofe. ......
....
The iifformalion In Hus bulletin is, to our beat knowledge, true and ', accurate, but all iVeommendalionH or suggestions are made without
guaranlee. ainoe the conditions of use are beyond our control. The Monsanto Chemical Company disclaims any liability incurred in
a,-IXx..'
.Ur/.'
' r-~--
~
if-- .
connection with the me of these data or suggestions,
Furthermore, nothing contained herein shall be construed as a recom-
mendution to use any product in conflict with existing patents covering
any material or its use.
. ad
'Fat -- -
-----...
..v.-.n
u,..... -- . .. .
WATER PCB-00034543
THE NEED FOR AROCLOR PJ.ASTICIZKRS
When incorporated into epoxy resin formulations, Aroclor compounds can be used to impart fire resistance; to increase flexibility; to improve processing; to maintain chemical resistance; to maintain adhesive characteristics and to lower finished product costs. The quality advantage of self-extinguishing epoxy compositions is of great interest in electrical, structural and coatings applications. Aroclor compounds are outstanding for providing fire retardancy since they offer the additional advantages of high chemical resist ance (inertness), resistance to water, acid and alkali extraction and very low per pound cost. Frequently, the addition.of Aroclor results in lower over-all finished product coots by their replacing a percentage of the higher cost ingredients.
SELECTED PROPERTIES OF AROCLOR COMPOUNDS
The Aroclor compounds, from Aroclor 1221 to Aroclor 5460, span a wide range of physical properties. Over the series, the properties vary in a regular gradient; giving a choice for optimum usefulness in any particular application. Adjustment of formulation properties can further be made by "blending" two or more Aroclor compounds to give a mixture for the specific use. The five* (of twelve) Aroclor compounds listed illustrate the variety of properties available.
* For a complete summary describing the properties of the entire
series of twelve Aroclor compounds, request a copy of "The Aroclor Compounds."
Address request to:
Monsanto Chemical Company
Organic Chemicals Division Dept. CS-14 800 N. Lindbergh Blvd. St. Louis 66, Missouri
.
Monsanto Chemical Specialties Data Report CS-14................................Page 2
0019 190
WATER PCB-00034544
TABLE I THE PROPERTIES OF ARCCLOR COMPOUNDS
Form
Aroclor 1221 Colorless mobile oil
Aroclor 1242 Practically
colorless mobile oil
Aroclor 1260 Light yellow soft sticky resin
Acidity - Maximum (Mgm.KOH per Gm.).............. .
0.015
0.015
0.015
Typical Density Specific Gravity 25/25C (77/77F)............. Lbs./Gallon-25C (77F)...
1.182 9.85
1.380 11.50
1.620 13-50
Distillation Range ASTM D-20 (Mod.) Corr. C......................................
275-320
325-360
385-420
Evaporation Loss - ASTM D-6 Mod. 163C - 5 hrs.......................... 100C - 6 hrs.......................... .
3.0 to 3.6 1.0 to 1.5 0.0 to 0.4
0.5 to 0.8 0.0 to 0.1
Flash Point Cleveland Open Cup-C.....
0F____.
I4l-150 286-302
176-180 348-356
None
Fire Point - Cleveland Open Cup - C..........................
F..........................
176 3^9
None* it
None tt
Pour Polnt-ASTM D-97-C..
F..
Softening Point -- ASTM E-28 - C......................
F........................
Crystals at 1C Crystals at 34F
-19 2
----
31 88
--
Refractive Index D-llne - 20C............
Vlsccsity-Saybolt Ur 210F (98.9c)................. 30F (54.4C)................. iCOT (37.8c).................
1.617-1.618 1.627-1.629
30-31
35-37 40-42
3^-35 49-56
80-93
1.647-1.649
72-78 3200-4500
--
1 None lndl cato3 ''Mo fire coint nri to boiling temperature.
Aroclor 1268
White opaque resin
Aroclor 5460 Yellow Trans parent resin
0.05
0.07
1.810 15-09
1.670 13.91
435-450
28o-335 at 5 mm. Hg.
0.1 to 0.2
0.03
0.0 to 0.6
1.5 to 1.7
(at 260-5 hrs.)
Non ne
NoII ne
None
..
No11 ne __
135 to 160 100to 105.50 (hold pt.) 275 to 320 212to 222 (hold pt.) .
1.660-1.665
--
--
WATER PCB-00034545
PROPERTY IMPROVEMENTS OF EPOXY FORMULATIONS
The Aroclor compounds represent one of the few plasticizer type materials that possess a high degree of compatibility with epoxy resins. The lower chlorinated members, 1221 and 1232, Impart a high degree of flexibility to epoxies while the more resinous and solid Aroclor compounds, e.g., 5460, have little flexibilizing effect, in fact, tend to act as reinforcing resins. Aroclor compounds, in general, have negligible influence on the hardness, tensile or compressive yield strength of epoxy resins. In phthallc anhydride cured systems, the ultimate compressive strengtn can even be improved by addition of'solid Aroclor compounds to the formulation.
When used in the range of 15 to 20 parts per hundred of resin, all of the Aroclor compounds greatly retard the burning rate of epoxy compositions. A small amount of antimony oxide added to the Aroclor formulations further increases the fire-retardance greatly and the epoxy formulations become non-burning. Aroclor creates self extinguishing characteristic; the antimony oxide functions to reduce afterglow. In addition, the antimony oxide can replace a portion of any fillers that may be employed.
Aroclor compounds are especially useful whenever finished product cost plus other specific qualities, such as good resistance to chemicals (especially acid and alkali), are Important factors. In surface coatings, for example, Aroclor 1254, 1260 and 1262 provide both formulating economy and excellent chemical resistance. However, Aroclor should not be used where maximum organic solvent resistance is desired since it is a true plasticizer and not chemically bound to the resin.
In potting compounds, Aroclor compounds can provide added flexi bility to improve the shock resistance of the encapsulated device. In addition, by proper selection of the Aroclor compound, the coating viscosity can be greatly reduced.
Better tackiness can be developed in epoxy adhesives by the "stickiness" property of Aroclor. In epoxy sealants, besides fire resistance, easier workability develops in the formulations.
Wherever fire-resistance, inertness, better flow and improved handling characteristics are needed, Aroclor compounds should be evaluated. Their unique properties and the effect on the epoxy resin as well as their low cost per pound recommend their evaluatlon for a variety of epoxy resin end uses.
LABORATORY DATA -- AROCLOR COMPOUNDS IN LIQUID EPOXY RESINS
The following data have been assembled as a guide for formulators of epoxy resins. Careful study of these data disclose several generalizations.
Monsanto Chemical Specialties Data Report CS-14...........................Page 4
WATER PCB-00034546
0019 192
The use of liquid Aroclor in an aliphatic amine-cured system -- 20 parts per 100 parts of resin basis -- results In a self-extinguishing formulation. Replacement of five parts of Aroclor with five parts of antimony oxide produces materials with still better flame retardancy. Flexural strength and compressive yield strength is improved while tensile strength remains unaffected. There is a slight lowering of heat distortion temperature and ultimate compressive strength.
In phthalic anhydride cured systems, solid Aroclor compounds greatly improve ultimate compressive strength, flexural strength and tensile properties. Compressive yield strength is comparable to the unplastlcized control while heat distortion temperature is lowered slightly
The liquid epoxy resins used in the experiments recorded in Table II are representative of commercial types such as Clba's Araldlte 6010, Jones and Dabney's EPI-Rez 510. Shell's Epon 828, Bakellte's ERL 2774 or Dow's DER 332.
Monsanto Chemical Specialties Data Report CS-14
00X9193
Page 5
WATER PCB-00034547
TABI TI AROCLOR IN LIQUID EPOXY RESIN
Formulation
Cure: 16 Hr. R. T. + 2 hrs.g 1QQC. _________20 Hrs. @ 150C.
Control
Modified
1 2 3 4 5b 7 8 9
Control 10
Liquid Epoxy Resin 100 100 100 100 100 ICO 100 100 100 100
Diethylene Triamine m 13 13 13 13 13 -
Aroolor 1260
o-
20 15
_
_
Aroclor 1242
s-
-
20 15 - _ _
Antimony Oxide
>> -
-
5-
5-
5_
5
Aroclor 1268
- - - - - 20 15
_
Aroclor 5^60
" - - - ...
20 15
Phthalic Anhydride Jj
-
-
-
-
- 75 75 75 75 75
DMP 30 (Rohm & Haas) ,
-
- - - .1 .1 .1 .1 .1
Flammability ASTM 635-56T
.82 in/ S. E. min. 1-1/8'
N.B. S.E. N.B. .38 in/ N.B. .38 in/ N.B. .6 in/
2-1/8"
min.
min.
min.
Heat Distortion Temp.
C. 117.5
87
92
79-5 81.0 128 134 135-5 135
143
Roclcwell "M"
104 103 106 108 1C7 112 112 113 111 111
Flex Strength PSI
20,000 23 ,800 22,100 21,800 22,200 25,900 20,000 26,300 19,000 16,900
Tensile PSI
11,400 13 ,000 9,8C0 10,700 12,800 13,500 11,100 11,500 10,200 11,000
Compressive Yield Strength PSI
15,700 17 ,250 16,950 17,900 16,700 22,300 20,500 21,000 21,200 20,900
Compressive Ultimate
Strength PSI
43,000 32,900 38,150 32,500 32,400 36,500 36,700 41,700 40,700 23,400
OOl^*
S. E. = Self extinguishing N.B. = No burning
WATER PCB-00034548
Table III Illustrates some other typical physical property modifl cations imparted by Aroclor 1221 and 1248. In each case, the formulation consisted of 100 parts epoxy resin (as in Table 11), 25 parts of Aroclor and 8 parts of tetraethylenepentamlne.
Compatibility
Liquid Room Temp. Cure 30 Min. Cure 100C.
TABLE III
Control
Compatible Compatible Compatible
Aroclor 1221
Compatible Compatible Compatible
Aroclor 1248
Compatible Compatible Compatible
VISCOSITY*
Before adding curing agent After adding curing agent
12,800 7,900
. 1,650 1,200
7,700 4, 300
PHYSICAL PROPERTIES**
Izod Impact Resistance Clarity: / light reflected Shore D Hardness (10 sec.)
0.2 3-0 78
_
3.0 8
0.6 3.0 40
PHYSICAL PROPERTIES AFTER HEAT AGING***
Shore D Hardness (10 sec.) % Weight Change
86 -0.012
81 -2.118
88 -0
* Brookfield LVF #4 spindle at 60 r.p.m. ** Samples cured 30 min. at 100C. with 8 p.hr. tetraethylenepentamlne
*** Aged 24 hours at 86C. in activated carbon
EFFECT OF CONCENTRATION OF ANTIMONY OXIDE AND AROCLOR ON FLAMMIBILITY
To determine the effective concentration of Antimony oxide and Aroclor (equal parts by weight), several test resin mixtures were prepared. Liquid epoxy resin (Shell Epikote 834) was mixed with Aroclor and antimony oxide and cured with 8% dlethylenetriamine. Specimens were prepared in wax molds 9"x x f". The flammibility tests were based upon the British Ministry of Supply Aircraft Specifications DTD 5537 Appendix 10. This procedure consisted of clamping the test specimen in a support with its longitudinal axis horizontal and its transverse axis inclined at 45. A bunsen burner was applied with the tip of the flame 1/2" to 3/4" just in contact with the end of the specimen. At the end - 30 seconds, the flame was removed and the specimen allowed to burn. If burning did not continue, the flame was replaced for 30 seconds and if the specimen again failed to continue burning, the material was classed as self-extinguishing. These results are listed in Table IV.
001919 b
Monsanto Chemical Specialties Data Report CS-14
Page 7
WATER PCB-00034549
TABLE IV AROCLOR AND ANTIMONY OXIDE (50-50 Mix)
Weight %
in Resin
Aroclor 1242
Aroclor 1260
Aroclor 4465
5
Inflammab]e
Inflammable
Inflammable
7.5
S.I.
S.I.
10 Inflammable S.E.
S.E.
(30 sec.)
(20 sec.)
15
S.E.
S.E.
S.E.
(30 sec.)
immediate
immediate
S.E. - Self-extinguishing S.I, - Semi-Inflammable
Aroclor 5460
Inflammable S.E.
(40 sec.)
S.E. (20 sec.)
S.E. immediate
************
For samples of the Aroclor products mentioned in this report, contact the nearest.branch office (see attached list) or write to:
MONSANTO CHEMICAL COMPANY Organic Chemicals Division Plasticizers Department 800 North Lindbergh St. Louis 66, Missouri
Monsanto Chemical Specialties Data Report CS-14
Page 8
WATER PCB-00034550
MONSANTO CHEMICAL COMPANY Organic Chemicals Division
District Sales Offices
ATLANTA: 1401 Peachtree St. N.E., Atlanta 5, Georgia
BOSTON: Everett Station, Boston 49, Massachusetts
,
CHICAGO: McGraw-Hill Building, 520 N. Michigan Ave., Chicago 11, 111.
CINCINNATI: 2330 Victory Parkway, Cincinnati 6, Ohio
CLEVELAND: 427 Hanna Building, Cleveland 15, Ohio
DETROIT: 18230 Grand River Avenue, Detroit 23, Michigan
HOUSTON: 2472 Bolsover St., P. 0. Box 6863, Houston, Texas
LOS ANGELES: 6670 E. Flotilla St., Los Angeles 22, California
MINNEAPOLIS: Foshay Tower, Room 515, Minneapolis 2, Minnesota
NEW YORK: 445 Park Avenue, New York 22, New York
PITTSBURGH: 20 Cedar Boulevard, Pittsburgh 28, Pennsylvania
SAN FRANCISCO: 111 Sutter Street, San Francisco 4, California
SEATTLE: 911 Western Avenue, Seattle 4, Washington
SYRACUSE: 731 James Street, Syracuse 3, New York
WILMINGTON: 2005 Concord Pike, Fairfax, Wilmington 3, Delaware
******
LONDON: Monsanto House, 10-18 Victoria St., London S.W. 1, England MELBOURNE: 256 Flinders Street, Adelaide, Australia MONTREAL: P. 0. Box 900, Montreal 3, Canada TORONTO: 183 Front St. East, Toronto 2, Ont., Canada VANCOUVER: 1550 Rand Avenue, Vancouver 14, B. C., Canada
0019197
i
Monsanto Chemical Specialties Data Report CS-14....................................... Page 9
WATER PCB-00034551