Document dYzXJKOe2Lrw1834E8JZr7pDQ

CSL-140A (Supersedes CSL-140) Report front the COATINGS SERVICE LABORATORY ADHESION OF LACQUERS TO ALUMINUM FOIL Requirements of good coatings for aluminum foil - adhesion, fastdry, flexibility, printability, and light stability -- can be obtained from lac quers based on nitrocellulose or ethyl cellulose. Adhesion is particularly difficult to achieve on aluminum because of the smooth, dense, impervious surface 02" the metal; and aluminum foil usually presents an even more difficult problem because the oil residues which have beers baked into the surface during processing are not usually removed. Thus, coatings that have good adhesion to untreated foil are rel atively uncommon. Good adhesion to untreated aluminum foil has been obtained in our laboratory with lacquers and inks based on Hercules Ethyl Cellulose and Nitrocellulose. This report presents results obtained from two programs; the first section covers studies made with nitrocellulose lacquers and the second reports studies with ethyl cellulose lacquers. ' A. ADHESION OF NITROCELLULOSE LACQUERS The Hercules Coatings Service Laboratory investigated the adhe sion of four nitrocellulose-based formulations to two types of untreated foil - "Reynolds Wrap" foil sold for household use, and a heavy-duty foil used as an overwrap on cigarette cartons. The coatings were, applied with a No. 150 band gra.vure roller, flash-dried a few seconds, then, force-dried 2 minutes at 180 "F. ' Nitrocellulose lacquers modified with a poly(vinyl acetate) resin were found to have strong adhesion to Reynolds Wrap. This untreated foil is particularly difficult to coat because a special oil, which causes poor adhesion of coating materials, is applied after processing to protect its surface (formulations Hi and H2 in Table I). These same lacquers, sur prisingly, had only fair adhesion to the foil used to overwrap cigarette cartons; here the processing oils were baked on the foil surface. Two other lacquers, onemodified with a polyamide and the other with Neolyn 23 resin (formulations H3 and #4 in Table 1), adhered to the overwXap foil surface more strongly than the commercial coating presently used. ' JIit-huk* w<- ciuimil anticipate or control the tunny different conditions under which tliu information sort pur products may be v.'r do not giiomnlrr the Applicability or llic accuracy of Ibis infornuilmn of the* loilability of our products in any given situation. Users of our products should make flicir ovk'o testy to dclrnnlnr the auilabilily of curb such product for their particular purposes. The products discussed an- told vilUou! such warranty, either express or implied, Also, tK(cn>cu concerning the possible use of oiu products aic not Intended m retoniinrndatiom to use our products in ih<- Infringement of any patrnL .......................................... ....... - ..............ftjQp. If?........ Q . A ..................... . ; ....... . . POLYMERS DEPARTMENT HERCULES POWDER, COMPANY WILMINGTON, DELAWARE M O N -M T -0 0 3 199 WATER_PCB HERCULES Technical Data CSL-140A Page 2 of 6 Table I ADHESION OF LACQUERS TO ALUMINUM FOIL Vehicle Solids j(a) 2u> 3 (a) 4(a) RS* Nitrocellulose, 1/2 sec. SS* Nitrocellulose, 1/2 sec. Polyfvinyl acetate) {Gelva V-25) Polyamide (Versamid 940) Neolyn 23 resin Dicyclohexyl phthalate Santicizer 141 -- 50 25 20 50 ' - 60 40 . - - - - - 36 - - 36 - 1^ 40 - '14 - - 14 - . Total 100 100 100 100 Physical Properties f 5cotch Tape adhesion' ' to: Reynolds Wrap, (untreated foil) \wJ G - . P' Untreated foil used for cigar- ette carton overwrap PpGG Shellac-treated foil p F. - G Blocking, 130 "F. 2 p. s. i. at 40 hr. Face-to-face B B NB NB Face-to-back NB NB NB NB 5_ bo C 0 u V0H r-i ri UH V rH+ rhH** 0 Q - F - - - * Hercules Trademark Legend: B = block; NB = no blocking; G = good; F = fair; P = poo.r. (a) Solvent Systems: Toluene Ethyl alcohol Ethyl acetate Butyl acetate For Formulations 1 & 2 43 17 13 27 . 100 For Formulation 3 50 20 15 15 100 For Formulation 4 - Dissolve Versamid 940 in a 50:50 mixture of toluene and ethyl alcohol. Add this solution to a nitrocelluloseplasticizer solution dissolved in solvent^), (b) Adhesion test method - Adhesion was tested by firmlypressing Scotch Brand Acetate Film Tape No. BOO on the coating. The tape was re moved by pulling it back at an angle of 180 Adhesion was noted a6: Good - no failure occurred when tape was removed abruptly^ Fair - failure occurred when tape was abruptly removed. No failure oc curred when tape was pulled back 6lowly. Poor - failure occurred when tape was removed slowly. Very poor -- no force was required to remove coating. MON-MT-003200 App k> TOWOLDMON0046325 WATER_PCB-00037302 I HERCULES Technical Data I CSL-140A Page 3 of 6 I B. ADHESION OF ETHYL CELLULOSE LACQUERS I Hercules Ethyl Cellulose N-10, modified with Aroclors 1254 and 5460 (lacquer $ 1, Table II), produced a coating having excellent adhesion and flexibility on both lightweight and heavy aluminum foil. Aging of the I lightweight coated foil6 for two months did not impair film adhesion prop erties. This formulation was at least as good as the betteT of two commer cial foil lacquers, on lightweight foil {Table IV), and superior to both on I heavy-gauge foil (Table V). Two other experimental lacquers (#4 and #6, Table II) had good to excellent initial adhesion on lightweight foil, about .equivalent to the better of the two commercial coatings. On two months' aging, however, some "loss of adhesion resulted (Table IV). On heavv-gauge foil, #6 lacquer was unsatisfactory, but $4 was somewhat better than the commercial products (Table V). " Special tests involved additions of 0. 25% phosphoric acid to deter mine if adhesion could be improved by the etching action of the acid on the foil. Little if any effect was observed (Tables IV and V). A report from the trade had previously stated that adhesion was ad versely affected by addition of certain dyes such as Calco Fast Spirit Red B. This report was not substantiated by these tests. .The most effective modifiers for improved foil lacquers based on ethyl cellulose were: 1. Aroclors 1254 and 5460. 2. Triphenyl phosphate and Resimene B81. ' Five experimental ethyl cellulose lacquers (# 1 through H5', Table II) were tested at 1-mil film thickness for initial adhesion and flexibility on lightweight aluminum foil. The results, compared with four commercially coated foils, were used to select most promising compositions Iot further testing. Results are'in Table HI. The two best lacquers (jj} and #4, Tables II and III) were coated along with a third composition ($6, Table I) in nominal film thickness of 0.2 mil on both lightweight and heavy-gauge aluminum foil. Results on lightweight foil are in Table IV, and on heavy-gauge foil in Table V. See page 6 for description of test methods used as reported in tR\se tables. ' MON-MT-003201 TOWOLDMON0046326 WATER_PCB-00037303 I I I I I 1 1 I r r I HERCULES Technical Data C5L- 140A Page 4 of 6 Method Of Film Casting On lightweight foil, the coatings were cast with a Hercules casting knife, air-dried 5 minutes, force-dried 5 minutes at 190 6F.., and airdried overnight. The heavy-gauge foil was dip-coated, air-dried 5-10 minutes, forcedried 5 minutes at .190 eF. , and air-dried overnight. . Table II ETHYL CELLULOSE LACQUER COMPOSITIONS FOR ALUMINUM- FOIL COATING Solids . 1 4>~r o 4 Hercules Ethyl Cellulose N-10 Hercules Ethyl Cellulose N-14 60 60 60 50 -- - - Aroclor 1254 20 - - - Aroclor 5460 . 20 - - - Super Beckacite No. 1001. Tricresyl phosphate Triphenyl phosphate Staybelite Ester No. 10 Santiciz.er B-16 Resimene 881 Paraplex RG-2 - 100 28 6 6 - 100 - 10 30 '100 - - 23 25 100 Solvent Xylene Toluene Isopropanol 80 80 - 80 -- 80 - 20 20 - 20 Ethyl acetate -- 20 - 5 50 - - - 25 25 100 80 20 V 50 - - - 40 10 100 80 20 . Table HI ' ETHYL CELLULOSE FILM PROPERTIES Commercially Lacquex No, Coated Foils Adhesion - Initial 1 2 345 12 3 4 Tape test (method A) E G GE F G G G G Fingernail test E E GE F G G G G Flexibility (180 crease at 75F. ) Initial 1 E E E E E .E E E E Nominal film thickness Aluminum foil gauge Lacquer solids, % 1 mir\ 0. 35-0, 40 mil 33 Legend: E = excellent, no effect; G = good, ve ry slight effect; F = fair, moderate effect; P = poor, noticeable effect. MON-JVfT- TOWOLDMON0046327 WATER_PCB-00037304 HERCULES Technical Data t CSL-140A Page 5 of 6 Table IV ETHYL CELLULOSE FILM PROPERTIES ON LIGHTWEIGHT FOIL Adhesion - Initial Tape test (method C) Lacquer additive - none acid^ dye W ------------------------------------------ --aci 4 dye(b) Adhesion - 2 Months Aging Tape test (method C) Lacquer additive - none acidU) ' dyeW acid^ dye (b) Lacquer Number 1 4s E EG E EE E EE E EG EP E pP E P G E .P p Commercial Lacquer XY F' G FE PE pP P E P TT PE Flexibility (I BO " crease at 75 F. Initial Aged 2 month Nominal film thickness Aluminum foil gauge Lacquer solids, % E EE E EE EE TT TT 0. 2 mil 0. 35-0. 40 mil 14-15.5 Legend: Same as in Table HI on page 4. (a) 0. 25% phosphoric acid based on lacquer solids. (b) 2, 6% Calco Fast Spirit Red B dye based on lacquer solids. Table V ETHYL CELLULOSE FILM PROPERTIES ON HEAVY-WEIGHT FOIL Adhesion -- Initial Tape test (method B except as noted) Lacquer additive - none acid^) dye^c) . acid^) + dye(c) Flexibility (180" crease at 75 F.) Initial ' Lacquer Number 1 46 E E jpv3-) E EP E EP E PP E EE Commercial XY G P(1 a) GPP E- EE Nominal film thickness Aluminum foil gauge Lacquer Bolide, % 0. 2 mil 3. 5-4,5 mi\s 14-15.5 ' Legend: E = excellent, no effect; G = good, very slight effect; F = fai:r 7 moderate effect; P - poor, noticeable effect. (a) Tape te6t method C. (\<pp u > (b) 0. 25% phosphoric acid based on lacquer solids. MOT tc) 2. 6% Calco Fast Soirit Red B dve based on laccuex eolids. .\o TOWOLDMON0046328 WATER PCB-00037305 HERCULES Technical Data CSE-140A Page 6 of 6 ( Vi ADHESION TEST METHODS Tape Test Method A Three inches of 1-inch wide Scotch Tape was applied and smoothed over the coated foil. After 30 to 60 seconds, it waB rapidly pulled away from the surface. Adhesion was estimated by noting the amount of lacquer removed by the Scotch Tape, Tape Test Method B Same as -Test A, except that a 1,000-gTam weight was rolled over the Tape after application. Tape Test Method C Same as Test A, except masking tape was used in place of Scotch Tape and a 200-gram weight was used. This method is not as severe a test as Method B. . Fingernail Test An area of the coated foil was crosshatched in approximately 1/8 to 3/16 inch squares with a razor blade. Adhesion was estimated by ease of removal when scratched with the fingernail. . I I ^' I . \ MON-MT-003204 A,pp b . thg 7 TOWOLDMON0046329 WATER_PCB-00037306